MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
LyondellBasell Hifax TYC 762P YGYA BLK Thermoplastic Olefinic Elastomer, mineral Filled
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Olefinic Elastomer (TPO)

Material Notes: Hifax polypropylene resins based on the Catalloy process are used in applications such as building and construction (e.g., single-ply roofing), industrial applications (e.g., wire and cable), and automotive industries. Hifax priovides good processability, excellent impact resistance, a broad range of stiffness from very soft to rigid products, high temperature resistance and low linear coefficient of thermal expansion.

Hifax TYC 762P YGYA BLK very high melt flow, 1,600 MPa flexural modulus, precolored, UV-stabilized, mineral-filled, paintable thermoplastic elastomeric olefin has an excellent balance of properties, processability, and paintability. It is typically used for automotive bumper fascias.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.03 g/ccISO 1183
Melt Flow 28 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 17.0 MPaISO 527-1,-2
Elongation at Yield 13 %ISO 527-1,-2
Flexural Modulus 1600 MPaISO 178
Izod Impact, Notched (ISO) 4.00 kJ/m²
@Temperature -40.0 °C
ISO 180
 30.0 kJ/m²
@Temperature 23.0 °C
ISO 180
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C
@Temperature -30.0 - 100 °C
ISO 11359-1,2
Deflection Temperature at 0.46 MPa (66 psi) 94.0 °Cunannealed; ISO 75B-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 56.0 °Cunannealed; ISO 75A-1,-2
 
Descriptive Properties
Processing MethodInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsubishi Iupiace® LGX420N m-Polyphenylene Ether (m-PPE)
MRC Polymers NAXELL™ PC23M-10G General Purpose Polycarbonate, 10% Glass Fiber Filled, Low Viscosity
LyondellBasell Hifax TYC735P 598F ANTHRACITE Thermoplastic Olefinic Elastomer, mineral Filled
LyondellBasell Hifax TYC735P 501F SMOKE Thermoplastic Olefinic Elastomer, mineral Filled
LyondellBasell Hifax TYC735P 207D CHARCOAL Thermoplastic Olefinic Elastomer, mineral Filled

PEQT7514 / 219151

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.