MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Versalis Clearflex® FG 336 A Film Grade LLDPE
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Hexene, Film Grade

Material Notes: Clearflex® FG 336 A is a hexane copolymer linear low density polyethylene (C6-LLDPE), with antioxidant, slip agent, antiblocking agent and processing aid, suitable for blown film extrusion. Films obtained from Clearflex® FG 336 A show high rigidity together with optimum Elmendorf tear and impact resistance.

Application: Clearflex® FG 336 A is recommended for shipping sacks, where the perfect balance between (in terms of slip and antiblocking) and mechanical performances leads to the manufacture of a tough and easy peel able film. Moreover, for its sealing characteristics, together with low temperature mechanical resistance, Clearflex® FG 336 A is suggested for the production of freezer bags, either in co extrusion and in blend with LDPE.

Property data reported for film extruded between 190°-230°C, with BUR 2.5, thickness 25 µm.

Information provided by Versalis.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.926 g/cc0.0335 lb/in³ISO 1183
Thickness 25.0 microns0.984 milAs tested
 10.0 - 50.0 microns0.394 - 1.97 milRecommended
Melt Flow 0.80 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.80 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 12.0 MPa1740 psiISO 527-3
Film Tensile Strength at Yield, TD 13.0 MPa1890 psiISO 527-3
Film Elongation at Break, MD 550 %550 %ISO 527-3
Film Elongation at Break, TD 740 %740 %ISO 527-3
Coefficient of Friction, Dynamic >= 0.11>= 0.11ISO 8295
Elmendorf Tear Strength, MD 8.40 g/micron213 g/milISO 6383-2
Elmendorf Tear Strength, TD 25.5 g/micron648 g/milISO 6383-2
Dart Drop Test 120 g0.265 lbF50; ISO 7765-1/A
Film Tensile Strength at Break, MD 45.0 MPa6530 psiISO 527-3
Film Tensile Strength at Break, TD 36.0 MPa5220 psiISO 527-3
1% Secant Modulus, MD 180 MPa26100 psiISO 527-3
1% Secant Modulus, TD 200 MPa29000 psiISO 527-3
 
Thermal PropertiesMetricEnglishComments
Melting Point 127 °C261 °FManufacturer method
Vicat Softening Point 110 °C
@Load 1.00 kg
230 °F
@Load 2.20 lb
ISO 306/A
Brittleness Temperature <= -70.0 °C<= -94.0 °FASTM D 746
 
Optical PropertiesMetricEnglishComments
Haze 13 %13 %ISO 14782
Gloss 54 %54 %45°; ASTM D 2457
 
Processing PropertiesMetricEnglishComments
Processing Temperature 190 - 230 °C374 - 446 °FAs Tested

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENF9829 / 265533

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.