MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Supradel® HTS-2420 High Temperature Sulfone Resin  (discontinued **)
Categories: Polymer; Thermoplastic; Polysulfone (PSU); Polysulfone, 20% Glass Fiber Reinforced

Material Notes: SUPRADEL HTS-2420 is a 20% glass-fiber reinforced high-temperature, high-performance, amorphous, sulfone polymer. With a glass transition temperature of 245°C and a heat deflection temperature of 240°C, SUPRADEL HTS-2420 resin this resin extends the thermal capability range available in other sulfone polymers.

The resin is completely amorphous and fully thermoplastic allowing easy melt fabrication by means of operations such as injection molding and extrusion. Along with its high thermal performance capabilities, SUPRADEL HTS-2420 resin also has a long list of high-performance attributes which include excellent hydrolytic stability, resistance to acids and bases, and inherent flame retardance.

SUPRADEL HTS-2420 resin is easily amenable to fabrication by injection molding, and other thermoplastic fabrication techniques. By virtue of its very high temperature performance and the unique combination of other engineering attributes, SUPRADEL HTS-2420 resin constitutes a good candidate for metal replacement as well as non-thermoplastic resin replacement in a wide range of engineering applications.

SUPRADEL HTS-2420 resin is available in natural and black.

Information provided by Solvay Advanced Polymers

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.46 g/ccASTM D792
Water Absorption 0.30 %At 24 hours; ASTM D570
Water Absorption at Saturation 1.3 %ASTM D570
Linear Mold Shrinkage 0.0040 cm/cmASTM D955
Melt Flow 11 g/10 min
@Load 5.00 kg,
Temperature 400 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 16500 psiASTM D638
Elongation at Break 3.0 %ASTM D638
Tensile Modulus 910000 psiASTM D638
Flexural Strength 25.5 ksiASTM D790
Flexural Modulus 880 ksiASTM D790
Izod Impact, Notched 1.40 ft-lb/inASTM D256
Izod Impact, Unnotched 13.0 ft-lb/inASTM D4812
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 464 °FAnnealed 0.125 inch thick specimen; ASTM D648
Glass Transition Temp, Tg 473 °F
 
Processing PropertiesOriginal ValueComments
Melt Temperature 390 - 410 °CStock Temperature
Mold Temperature >= 180 °C
 190 - 210 °CLong flow or thin wall parts or for low residual stress
Drying Temperature 150 °C2.5 hours for injection molding
 170 °C> 4 hours hopper drying with desiccated air inlet for extrusion

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL92 / 67931

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.