MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Haynes Ultimet® alloy, aged 1000 hours at 316°C
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptional ductility and resistance to weld cracking, very easy to apply as an overlay, multiple layers appliable with little to no preheat. Applications include agitators, blenders, bolts, dies, extruders, fan blades, filters, glass plungers, nozzles, pumps, rolls, screw conveyors, and valve parts.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: DIN CoCr26Ni9Mo5W No. 2.4681, NACE MR0175-94 Section 4.1.6.3, UNS R31233, ASTM B-815, ASTM B-818
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.47 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 1069 MPa
Tensile Strength, Yield 552 MPa
@Strain 0.2 %
Elongation at Break 47 %in 50.8 mm
Modulus of Elasticity 180 GPa
@Temperature 649 °C
(heat treated at 1121°C (2050°F), water quenched plate)
 189 GPa
@Temperature 538 °C
(heat treated at 1121°C (2050°F), water quenched plate)
 197 GPa
@Temperature 427 °C
(heat treated at 1121°C (2050°F), water quenched plate)
 206 GPa
@Temperature 316 °C
(heat treated at 1121°C (2050°F), water quenched plate)
 215 GPa
@Temperature 204 °C
(heat treated at 1121°C (2050°F), water quenched plate)
Charpy Impact 217 J
@Temperature 23.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000870 ohm-cm
@Temperature 23.0 °C
 0.0000890 ohm-cm
@Temperature 100 °C
 0.0000930 ohm-cm
@Temperature 200 °C
 0.0000960 ohm-cm
@Temperature 300 °C
 0.000100 ohm-cm
@Temperature 400 °C
 0.000103 ohm-cm
@Temperature 500 °C
 0.000105 ohm-cm
@Temperature 600 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.0 µm/m-°C
@Temperature 26.0 - 316 °C
 14.5 µm/m-°C
@Temperature 26.0 - 427 °C
 14.8 µm/m-°C
@Temperature 26.0 - 538 °C
 15.1 µm/m-°C
@Temperature 26.0 - 649 °C
 15.9 µm/m-°C
@Temperature 26.0 - 760 °C
 16.4 µm/m-°C
@Temperature 26.0 - 871 °C
 16.9 µm/m-°C
@Temperature 26.0 - 982 °C
Specific Heat Capacity 0.456 J/g-°C
@Temperature 23.0 °C
 0.470 J/g-°C
@Temperature 100 °C
 0.482 J/g-°C
@Temperature 200 °C
 0.504 J/g-°C
@Temperature 300 °C
 0.525 J/g-°C
@Temperature 400 °C
 0.545 J/g-°C
@Temperature 500 °C
 0.573 J/g-°C
@Temperature 600 °C
Thermal Conductivity 12.3 W/m-K
@Temperature 23.0 °C
 13.8 W/m-K
@Temperature 100 °C
 15.6 W/m-K
@Temperature 200 °C
 17.5 W/m-K
@Temperature 300 °C
 19.4 W/m-K
@Temperature 400 °C
 21.5 W/m-K
@Temperature 500 °C
 23.9 W/m-K
@Temperature 600 °C
Melting Point 1332 - 1354 °C
Solidus 1332 °C
Liquidus 1354 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.060 %
Chromium, Cr 26 %
Cobalt, Co 54 %As Balance
Iron, Fe 3.0 %
Manganese, Mn 0.80 %
Molybdenum, Mo 5.0 %
Nickel, Ni 9.0 %
Nitrogen, N 0.080 %
Silicon, Si 0.30 %
Tungsten, W 2.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kennametal Stellite ULTIMET Cobalt Alloy
Haynes Ultimet® alloy, plate, GMAW weld (short)
Haynes Ultimet® alloy, all-weld metal, SMAW weld
Haynes Ultimet® alloy, all-weld metal, GMAW weld (short)
Haynes Ultimet® alloy, aged 1000 hours at 982°C

NHAUAX / 16966

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.