MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ovako 25CrMo4 322D Steel, Hardening
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 9000 Series Steel

Material Notes: General Information: Grade Ovako 322A and 322D are Cr and Mo alloyed quench and tempering steel with low carbon content. The steel combine high strength with high toughness.
  • Variant 322A correspond to the EN grade 25CrMo4.
  • Variant 322D corresponds to SAE 4130 / 30CrMo4*. Suitable for flame or induction hardening.
  • Variant 6014 is EN grade 25CrMo4 M-steel
Delivered as rolled, soft annealed normalized or quench and tempered. Weldable under certain conditions.

Information provided by Ovako

Key Words: 9224 - 27CrMo4-2, 30CrMo4*, 30CrMo4, SS2225, 4130
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 225
@Thickness <=25.0 mm
Tube, wall
 225
@Thickness <=25.0 mm
Tube, wall
 225
@Thickness <=25.0 mm
Tube, wall
Tensile Strength 730 MPa
@Thickness <=25.0 mm
Tube, wall
 730 MPa
@Thickness <=25.0 mm
Tube, wall
 730 MPa
@Thickness <=25.0 mm
Tube, wall
Tensile Strength, Yield >= 600 MPa
@Thickness <=25.0 mm
Tube, wall
 >= 600 MPa
@Thickness <=25.0 mm
Tube, wall
 >= 600 MPa
@Thickness <=25.0 mm
Tube, wall
Elongation at Break 23 %
@Thickness <=25.0 mm
Tube, wall
 23 %
@Thickness <=25.0 mm
Tube, wall
 23 %
@Thickness <=25.0 mm
Tube, wall
Reduction of Area 23 %
@Thickness <=25.0 mm
Tube, wall
 23 %
@Thickness <=25.0 mm
Tube, wall
 236 %
@Thickness <=25.0 mm
Tube, wall
Modulus of Elasticity 210 GPa
Poissons Ratio 0.30
Shear Modulus 80.0 GPa
Impact Test 176 J
@Thickness <=25.0 mm,
Temperature -40.0 °C
Tube, wall
 182 J
@Thickness <=25.0 mm,
Temperature -20.0 °C
Tube, wall
 193 J
@Thickness <=25.0 mm,
Temperature 20.0 °C
Tube, wall
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
Thermal Conductivity 40.0 - 45.0 W/m-KAmbient temperature
Transformation Temperature 391 °CMS
 746 °CAC1
 826 °CAC3
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.28 - 0.33 %
Chromium, Cr 0.90 - 1.1 %
Iron, Fe 97.09 - 98.04 %As Balance
Manganese, Mn 0.40 - 0.60 %
Molybdenum, Mo 0.18 - 0.25 %
Nickel, Ni <= 0.25 %
Phosphorus, P <= 0.025 %
Silicon, Si 0.20 - 0.35 %
Sulfur, S <= 0.010 %
 
Descriptive Properties
WeldabilityCEV 0.74max
 Pcm 0.47max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ovako 25CrMo4 322A Steel, Hardening
Ovako 25CrMo4 9224 Steel, Hardening
AISI 4130 Steel, water quenched 855°C (1570°F), 480°C (900°F) temper, 25 mm (1 in.) round
AISI 4130 Steel, water quenched 855°C (1570°F), 480°C (900°F) temper, 13 mm (0.5 in.) round
Ovako 25CrMo4 6014, MoC 210 M Steel, Hardening

NOVAKO201 / 234500

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.