MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Nylon 66, Glass/Mineral Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass/Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Glass/Mineral Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.23 - 1.73 g/ccAverage value: 1.45 g/cc Grade Count:180
 1.20 - 1.30 g/cc
@Temperature 245 - 295 °C
Average value: 1.26 g/cc Grade Count:4
Filler Content 10.0 - 45.0 %Average value: 31.8 % Grade Count:40
Water Absorption 0.350 - 6.00 %Average value: 1.36 % Grade Count:73
Moisture Absorption at Equilibrium 0.700 - 2.00 %Average value: 1.42 % Grade Count:19
Viscosity 30.0 - 120 cP
@Temperature 280 - 300 °C
Average value: 70.7 cP Grade Count:1
 30.0 - 120 cP
@Shear Rate 100 - 1000 1/s
Average value: 70.7 cP Grade Count:1
Maximum Moisture Content 0.0200 - 0.200Average value: 0.127 Grade Count:9
Linear Mold Shrinkage 0.000500 - 0.0500 cm/cmAverage value: 0.00596 cm/cm Grade Count:136
Linear Mold Shrinkage, Transverse 0.00100 - 0.0140 cm/cmAverage value: 0.00874 cm/cm Grade Count:56
Melt Flow 2.00 - 44.4 g/10 minAverage value: 22.5 g/10 min Grade Count:10
Ash 20.0 - 48.0 %Average value: 37.3 % Grade Count:6
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 74.0 - 99.0Average value: 96.4 Grade Count:15
Hardness, Rockwell R 112 - 122Average value: 120 Grade Count:34
Tensile Strength, Ultimate 50.0 - 195 MPaAverage value: 116 MPa Grade Count:137
 25.0 - 70.0 MPa
@Temperature 60.0 - 150 °C
Average value: 43.8 MPa Grade Count:2
Tensile Strength, Yield 71.7 - 175 MPaAverage value: 118 MPa Grade Count:48
Elongation at Break 1.00 - 160 %Average value: 4.24 % Grade Count:172
 2.70 - 20.0 %
@Temperature 60.0 - 150 °C
Average value: 8.90 % Grade Count:2
Elongation at Yield 2.00 - 6.00 %Average value: 3.76 % Grade Count:6
 5.00 - 10.0 %
@Temperature 90.0 - 150 °C
Average value: 7.33 % Grade Count:1
Modulus of Elasticity 3.30 - 15.5 GPaAverage value: 8.28 GPa Grade Count:59
 2.60 - 8.00 GPa
@Temperature 60.0 - 150 °C
Average value: 4.29 GPa Grade Count:2
Flexural Yield Strength 90.0 - 285 MPaAverage value: 177 MPa Grade Count:149
Flexural Modulus 2.90 - 12.5 GPaAverage value: 7.56 GPa Grade Count:170
Compressive Yield Strength 138 - 255 MPaAverage value: 187 MPa Grade Count:5
Poissons Ratio 0.340 - 0.400Average value: 0.352 Grade Count:8
Izod Impact, Notched 0.300 - 1.33 J/cmAverage value: 0.540 J/cm Grade Count:89
 0.420 - 0.420 J/cm
@Temperature -40.0 - -40.0 °C
Average value: 0.420 J/cm Grade Count:1
Izod Impact, Unnotched 0.427 - 9.08 J/cmAverage value: 5.06 J/cm Grade Count:31
 5.50 - 5.50 J/cm
@Temperature -40.0 - -40.0 °C
Average value: 5.50 J/cm Grade Count:1
Izod Impact, Notched (ISO) 2.60 - 42.0 kJ/m²Average value: 7.29 kJ/m² Grade Count:66
 3.00 - 10.0 kJ/m²
@Temperature -40.0 - -30.0 °C
Average value: 5.52 kJ/m² Grade Count:13
Izod Impact, Unnotched (ISO) 4.00 - 55.0 kJ/m²Average value: 35.2 kJ/m² Grade Count:6
 3.40 - 50.0 kJ/m²
@Temperature -40.0 - -30.0 °C
Average value: 35.9 kJ/m² Grade Count:6
Charpy Impact Unnotched 2.00 - 9.00 J/cm²Average value: 4.89 J/cm² Grade Count:36
 2.00 - 6.00 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 4.28 J/cm² Grade Count:20
Charpy Impact, Notched 0.200 - 1.60 J/cm²Average value: 0.617 J/cm² Grade Count:72
 0.200 - 1.00 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 0.464 J/cm² Grade Count:26
Tensile Creep Modulus, 1 hour 2300 - 7000 MPaAverage value: 5100 MPa Grade Count:3
Tensile Creep Modulus, 1000 hours 1500 - 6000 MPaAverage value: 3730 MPa Grade Count:3
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+9 - 1.00e+17 ohm-cmAverage value: 2.69e+15 ohm-cm Grade Count:46
Surface Resistance 1.00e+10 - 5.00e+14 ohmAverage value: 7.46e+13 ohm Grade Count:15
Dielectric Constant 3.00 - 13.9Average value: 4.82 Grade Count:14
Dielectric Strength 15.7 - 41.0 kV/mmAverage value: 25.4 kV/mm Grade Count:35
Dissipation Factor 0.0100 - 0.540Average value: 0.0642 Grade Count:8
Dielectric Loss Index 0.0150 - 0.150Average value: 0.0825 Grade Count:4
Arc Resistance 125 - 140 secAverage value: 130 sec Grade Count:5
Comparative Tracking Index 375 - 600 VAverage value: 439 V Grade Count:14
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.0 - 55.8 µm/m-°CAverage value: 29.6 µm/m-°C Grade Count:34
 31.0 - 31.0 µm/m-°C
@Temperature 55.0 - 160 °C
Average value: 23.2 µm/m-°C Grade Count:1
 18.5 - 24.0 µm/m-°C
@Temperature 35.0 - 55.0 °C
Average value: 23.2 µm/m-°C Grade Count:2
 18.5 - 24.0 µm/m-°C
@Thickness 2.00 - 2.00 mm
Average value: 23.2 µm/m-°C Grade Count:2
CTE, linear, Transverse to Flow 46.0 - 100 µm/m-°CAverage value: 73.5 µm/m-°C Grade Count:10
 127 - 127 µm/m-°C
@Temperature 55.0 - 160 °C
Average value: 127 µm/m-°C Grade Count:1
Specific Heat Capacity 1.90 - 2.29 J/g-°C
@Temperature 245 - 295 °C
Average value: 2.14 J/g-°C Grade Count:4
Thermal Conductivity 0.350 - 0.504 W/m-KAverage value: 0.427 W/m-K Grade Count:4
 0.210 - 0.270 W/m-K
@Temperature 245 - 295 °C
Average value: 0.248 W/m-K Grade Count:4
Melting Point 220 - 275 °CAverage value: 259 °C Grade Count:92
Maximum Service Temperature, Air 115 - 254 °CAverage value: 179 °C Grade Count:5
Deflection Temperature at 0.46 MPa (66 psi) 203 - 260 °CAverage value: 249 °C Grade Count:84
Deflection Temperature at 1.8 MPa (264 psi) 70.0 - 257 °CAverage value: 223 °C Grade Count:159
Vicat Softening Point 200 - 255 °CAverage value: 238 °C Grade Count:13
Glass Transition Temp, Tg 70.0 - 90.0 °CAverage value: 80.0 °C Grade Count:4
Flammability, UL94 HB - V-0Grade Count:59
Flame Spread 0.000 - 80.0 mm/minAverage value: 47.3 mm/min Grade Count:7
Oxygen Index 24.0 - 36.0 %Average value: 28.5 % Grade Count:4
Glow Wire Test 650 - 960 °CAverage value: 768 °C Grade Count:5
 
Processing PropertiesOriginal ValueComments
Processing Temperature 260 - 300 °CAverage value: 285 °C Grade Count:14
Nozzle Temperature 254 - 310 °CAverage value: 280 °C Grade Count:33
Melt Temperature 220 - 310 °CAverage value: 283 °C Grade Count:80
Mold Temperature 26.7 - 121 °CAverage value: 85.7 °C Grade Count:89
Drying Temperature 60.0 - 130 °CAverage value: 83.6 °C Grade Count:61
Moisture Content 0.0300 - 0.200 %Average value: 0.178 % Grade Count:34
Injection Pressure 3.50 - 138 MPaAverage value: 83.0 MPa Grade Count:28

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, Unreinforced
Overview of materials for Nylon 6, Glass/Mineral Reinforced
3M S38HS Glass Bubbles
3M S38 Glass Bubbles
3M S35 Glass Bubbles

O2538 / 78032

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.