MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
TIMET TIMETAL® 6-4 ELI Titanium Alloy (Ti-6Al-4V ELI; ASTM Grade 23) (Annealed; <3.0 in Rod or Thickness; Per ASTM B348)
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Beta Titanium Alloy

Material Notes: Medium To High Strength General-Purpose Alloy Minimum tensile property data below are specific to this MatWeb entry; other specific form/thickness entries are also available in MatWeb.

Features: A lower strength version of TIMETAL 6-4 with improved toughness, cryogenic ductility, and SCC resistance. Major uses are in the medical implant field, marine structural components, and oil and gas production. This variant is available for fracture critical applications. This alloy is available in most common product forms including billet, bar, wire, plate, and sheet.

Data provided by TIMET.

Key Words: Titanium 6-4 ELI; UNS R56401
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.42 g/ccTypical
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate >= 828 MPaLongitudinal
Tensile Strength, Yield >= 759 MPa
@Strain 0.2 %
Longitudinal
Elongation at Break >= 10 %Longitudinal
Reduction of Area >= 25 %Longitudinal
Modulus of Elasticity 95.0 - 111 GPa
@Temperature 230 °C
varies with heat treatment and texture
 107 - 122 GPa
@Temperature 20.0 °C
varies with heat treatment and texture
Poissons Ratio 0.31
Shear Modulus 41.0 - 45.0 GPa
Bend Radius, Minimum 5.0 t
@Thickness 2.00 mm
Typical; sheet
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000168 ohm-cm
 0.000168 ohm-cm
@Temperature 0.000 °C
 0.000186 ohm-cm
@Temperature 315 °C
 0.000189 ohm-cm
@Temperature 650 °C
Magnetic Permeability 1.00005at 20 Oersted
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.00 µm/m-°C
@Temperature 0.000 - 100 °C
 9.40 µm/m-°C
@Temperature 20.0 - 425 °C
 9.70 µm/m-°C
@Temperature 20.0 - 650 °C
Specific Heat Capacity 0.580 J/g-°C
@Temperature 20.0 °C
 0.670 J/g-°C
@Temperature 425 °C
 0.930 J/g-°C
@Temperature 870 °C
Thermal Conductivity 6.60 W/m-K
@Temperature 20.0 °C
 10.6 W/m-K
@Temperature 315 °C
 17.5 W/m-K
@Temperature 650 °C
Melting Point <= 1660 °C
Liquidus >= 1636 °C
 1660 °C
Maximum Service Temperature, Air 350 °CReasonable mechanical properties retained
Beta Transus 982 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 5.5 - 6.5 %
Carbon, C <= 0.080 %
Hydrogen, H <= 0.0125 %
Iron, Fe <= 0.25 %
Nitrogen, N <= 0.030 %
Other, each <= 0.10 %
Other, total <= 0.40 %
Oxygen, O <= 0.13 %
Titanium, Ti 88.1 - 91 %Calculated as remainder
Vanadium, V 3.5 - 4.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
TIMET TIMETAL® 6-4 ELI Titanium Alloy (Ti-6Al-4V ELI; ASTM Grade 23) (Solution Treated; 0.025 - 1.000 in Sheet and Plate; Per ASTM B265)
Titanium Ti-6Al-4V ELI (Grade 23), Annealed
Titanium Ti-6Al-4V (Grade 5), Annealed
Titanium Ti-6Al-4V (Grade 5), STA
TIMET TIMETAL® 21S Titanium Alloy (Ti-15Mo-3Nb-3Al-0.2Si, ASTM Grade 21); ST 1500°F (816°C) + Age 1000°F (538°C)

NTIMEELIB / 19343

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.