MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Celanese VECTRA FIT72 LCP, 35% Mineral / Glass Reinforced
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), 40% Glass Fiber Filled

Material Notes: 35% glass and mineral reinforced grade. It offers ultrahigh flowability, low warpage, and good mechanical property.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.65 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.00050 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0043 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 110 MPa50mm/min; ISO 527-2/1A
Elongation at Break 2.0 %50mm/min; ISO 527-2/1A
Tensile Modulus 12000 MPa50mm/min; ISO 527-2/1A
Flexural Strength 140 MPaISO 178
Flexural Modulus 12000 MPaISO 178
Flexural Strain at Break 2.5 %ISO 178
Charpy Impact Unnotched 30.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 8.00 kJ/m²ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 8.00 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 43.0 µm/m-°CISO 11359-2
Melting Point 331 °C10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 284 °CISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 240 °CISO 75-1, -2
 
Processing PropertiesOriginal ValueComments
Processing Temperature 80.0 - 130 °Ccavity
Zone 1 315 - 325 °C
Zone 2 325 - 335 °C
Zone 3 330 - 350 °C
Zone 4 330 - 350 °C
Die Temperature 330 - 340 °C
Melt Temperature 335 - 345 °C
Drying Temperature 150 - 170 °C
Dry Time 6.00 hour
Moisture Content <= 0.010 %
Injection Pressure 50.0 - 150 MPa
Screw Speed 100 rpm
@Diameter 40.0 mm
 140 rpm
@Diameter 25.0 mm
 200 rpm
@Diameter 16.0 mm
 
Descriptive Properties
Injection speedmedium-fast

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Thermx® CG933 PCT, 30% Glass Reinforced
Celanese VECTRA C130 LCP, 30% Glass Reinforced
Celanese VECTRA V143XL LCP, 42% Glass Reinforced
Celanese VECTRA S625 LCP, 25% Specialty

PHCQ515 / 178970

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.