MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Torlon® 7130 PAI, 30% carbon fiber
Categories: Polymer; Thermoplastic; Polyamide-imide (PAI)

Material Notes: 30% carbon fiber, best stiffness, best retention of stiffness at high temperatures, best fatigue resistance, electrically conductive

Torlon® 7130 is an 30% carbon-fiber reinforced grade of polyamide-imide (PAI) resin. It offers high strength and modulus, exceptional creep resistance, and good fatigue resistance. It has thermal expansion characteristics similar to steel, and therefore excellent dimensional stability.

Torlon® PAI has the highest strength and stiffness of any thermoplastic up to 275°C (525°F). It has outstanding resistance to wear, creep, and chemicals.

The potential applications for this resin include metal replacement, sliding vanes, aerospace parts, impellors, shrouds, pistons, and housings.

It is available in injection molding and extrusion (E) grades.

Markets/Uses: Aircraft / Mechanical & Structural Applications / Brackets and Hinges; Aircraft / Mechanical & Structural Applications / Engine Components; Aircraft / Mechanical & Structural Applications / Engine Fan Cowling Vents; Aircraft / Mechanical & Structural Applications / Fan Impeller; Aircraft / Mechanical & Structural Applications / Mounting Support Rails; Aircraft / Mechanical & Structural Applications / Seals; Aircraft / Mechanical & Structural Applications / Stock Shapes for Prototyping; Aircraft / Mechanical & Structural Applications / Support Brackets; Automotive / Mechanical & Structural Parts / Gears; Films / High Temperature Films / Brackets and Hinges; Films / High Temperature Films / Engine Components; Films / High Temperature Films / Engine Fan Cowling Vents; Films / High Temperature Films / Fan Impeller; Films / High Temperature Films / Mounting Support Rails; Films / High Temperature Films / Seals; Films / High Temperature Films / Stock Shapes for Prototyping; Miscellaneous / Industrial / Compressor Components; Oil & Gas / Down Hole / Back-Up Seal Rings; Oil & Gas / Down Hole / Compressor Components; Oil & Gas / Down Hole / Down Hole Connectors; Oil & Gas / Down Hole / Electrical Connectors; Oil & Gas / Down Hole / Motor End Plate; Oil & Gas / Down Hole / Poppets; Semiconductor / Fabrication & Testing / Mechanical Fasteners

Applications: Aerospace Applications; Aircraft Applications; Business Equipment; Connectors; Electrical/Electronic Applications; Film; Gears; Housings; Industrial Applications; Industrial Parts; Machine/Mechanical Parts; Metal Replacement; Oil/Gas Applications; Semiconductor Molding Compounds

Features: Chemical Resistant; Creep Resistant; Fatigue Resistant; Flame Retardant; Good Compressive Strength; Good Dimensional Stability; High Heat Resistance; High Stiffness; High Temperature Strength; Semi Conductive

Injection notes: Minimum drying conditions: 3 hours at 350°F (177°C), 4 hours at 300°F (149°C), or 16 hours at 250°F (121°C).
Compression Ratio: 1:1 to 1.5:1
Begin hold pressure at a high setting 6,000-8,000 psi (41.37-55.16 MPa), for several seconds, then drop off to 3,000-5,000 psi (20.69-34.48 MPa), for the duration of the hold pressure sequence.
Molded parts must be post cured.

Information provided by Solvay Specialty Polymers.

Vendors: Drake extrudes shapes and machines and injection molds parts in Torlon® PAI, PEEK, PAEK, Ryton PPS and Ultem PEI. It also machines Vespel® PI. Innovations include cryogenic CryoDyn® CT-200 shapes as a PCTFE alternative; efficient Seamless Tube® and the largest extruded rod diameters to >254mm and plate thicknesses to > 100mm. Certified to ISO 9001:2015 and AS9100D. Visit www.DrakePlastics.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.48 g/ccASTM D792
Water Absorption 0.26 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow <= 0.0015 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 221 MPaASTM D638
Tensile Stress 203 MPaASTM D1708
Tensile Modulus 16500 - 22300 MPaASTM D638
Flexural Strength 350 MPaASTM D790
Flexural Modulus 15700 MPa
@Temperature 232 °C
ASTM D790
 19900 MPa
@Temperature 23.0 °C
ASTM D790
Compressive Strength 254 MPaASTM D695
Compressive Modulus 9860 MPaASTM D695
Izod Impact, Notched 48.0 J/mASTM D256
Izod Impact, Unnotched 320 J/mASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 90.0 µm/m-°CASTM D696
Thermal Conductivity 0.520 W/m-KASTM C177
Deflection Temperature at 1.8 MPa (264 psi) 282 °CUnannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 304 °C
Nozzle Temperature 371 °C
Mold Temperature 199 - 216 °C
Drying Temperature 177 °C
@Time 10800 sec
Moisture Content <= 0.050 %Injection
Back Pressure 6.89 MPa
Screw Speed 50 - 100 rpm
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
FormsPellets
ProcessingInjection Molding; Machining; Profile Extrusion
RoHS ComplianceYes
Screw L/D Ratio, Injection18.0:1.0 to 24.0:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4552 / 280352

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.