MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Beijing Chemical Industry KAIFA® GL4200 ABS Thermal Resistant Grade
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Excellent thermal resistance

Information provided by Beijing Chemical Industry Research Institute (Group)

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³ASTM D792
Water Absorption 0.30 %0.30 %24 hr; ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 45.0 MPa6530 psiASTM D638
Elongation at Break 25 %25 %ASTM D638
Flexural Strength 73.0 MPa10600 psiASTM D790
Flexural Modulus 2.10 GPa305 ksiASTM D790
Izod Impact, Notched 0.150 J/cm
@Thickness 3.20 mm
0.281 ft-lb/in
@Thickness 0.126 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 103 °C217 °FASTM D648
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 - 230 °C356 - 446 °FResin Temp.
Rear Barrel Temperature 190 °C374 °F
Middle Barrel Temperature 210 °C410 °F
Front Barrel Temperature 220 °C428 °F
Nozzle Temperature 215 °C419 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
Drying Temperature 80.0 - 90.0 °C
@Thickness 30.0 mm
176 - 194 °F
@Thickness 1.18 in
Dry Time 4 hour
@Thickness 30.0 mm
4 hour
@Thickness 1.18 in
Injection Pressure 80.0 - 130 MPa11600 - 18900 psiinjection speed: 80 - 120 rpm
Back Pressure 1.00 - 2.00 MPa145 - 290 psiMold Pressure
Screw Speed 100 rpm100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Edinburg Plastics AGG625 ABS
INEOS Styrolution Terblend® N NMX04 ABS/PA6 (Dry)
INEOS Styrolution Terluran® HI-12 ABS
INEOS Styrolution Novodur® H604 ABS
Ineos ABS Lustran® 1465, Injection Grade

PKAIF69 / 48651

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.