MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Aluminum Bronze D, UNS C61400, H04 Temper 25 mm rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Good hot and cold formability.

Applications: nuts, bolts, stringers and threaded members, corrosion resistant vessels and tanks, structural components, machine parts, condenser tube and piping systems, marine protective sheathing and fasteners, munitions mixing troughs and blending chambers.

Test specimen: rod - 25mm diameter.

Key Words: CDA 614
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.89 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 84 - 91
Tensile Strength, Ultimate 565 MPa
@Strain 0.5 %
Tensile Strength, Yield 275 MPaIn 50 mm
Elongation at Break 35 %
Modulus of Elasticity 115 GPa
Compressive Strength 860 MPa
Poissons Ratio 0.312
Fatigue Strength 180 MPa
@# of Cycles 1.00e+8
Reverse Bending; Temper Not Reported
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 44.0 GPa
Shear Strength 310 MPa
Izod Impact 54.0 - 61.0 JTemper not specified
Charpy Impact 81.0 - 88.0 JKeyhole, temper not reported
 41.0 J
@Temperature 550 °C
cold finished (specific temper not reported)
 58.0 J
@Temperature 425 °C
cold finished (specific temper not reported)
 85.0 J
@Temperature 320 °C
cold finished (specific temper not reported)
 90.0 J
@Temperature 200 °C
cold finished (specific temper not reported)
 95.0 J
@Temperature -175 °C
cold finished (specific temper not reported)
 104 J
@Temperature -50.0 °C
cold finished (specific temper not reported)
 106 J
@Temperature 0.000 °C
cold finished (specific temper not reported)
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000123 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.375 J/g-°C
Thermal Conductivity 56.5 W/m-K
Melting Point 1040 - 1045 °C
Solidus 1040 °C
Liquidus 1045 °C
Annealing Point 1125 - 1650 °F
 
Processing PropertiesOriginal ValueComments
Processing Temperature 1010 °CHot-Shortness Temperature
Annealing Temperature 600 - 900 °C
Hot-Working Temperature 800 - 925 °C
Recrystallization Temperature 785 - 870 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 6.0 - 8.0 %
Copper, Cu 88 - 92.5 %
Iron, Fe 1.5 - 3.5 %
Lead, Pb <= 0.010 %
Manganese, Mn <= 1.0 %
Other, total <= 0.50 %
Phosphorus, P <= 0.015 %
Zinc, Zn <= 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum Bronze D, UNS C61400, H04 Temper 13 mm rod
Copper, UNS C62400 (Aluminum Bronze 11%), H50 Temper, 25 mm rod
Nickel Aluminum Bronze, UNS C63200
Alpha Nickel-Aluminum Bronze, UNS C95800, Copper Casting Alloy
Aluminum Bronze D, UNS C61400, Annealed Rod

MC61400c2 / 11590

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.