MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Wellman EcoLon® MRGF1518-BK Mineral/Glass Fiber Reinforced Nylon 66, Lubricated, Heat Stabilized, PCR  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass/Mineral Filled

Material Notes: Typical Applications: Lawn and garden equipment, automotive trim, bezels, wheel covers, window frames, gas tank filler housings, brackets, metalized lighting reflectors for automotive, automotive cooling fans & shrouds, automotive door handles, brackets, automotive mirror shells, painted parts, components for small gas engines, sporting goods, auto luggage rack components.

Data provided by the manufacturer, Wellman Inc.

Key Words: Polyamide 66
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.45 g/ccISO 1183
Water Absorption 0.60 %Approximate 24 hr.
Linear Mold Shrinkage 0.0060 - 0.010 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 100 MPaISO 527
Elongation at Break 3.0 %ISO 527
Flexural Yield Strength 155 MPaISO 178
Flexural Modulus 6.70 GPaISO 178
Izod Impact, Notched 0.400 J/cmISO 180
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 220 °CISO 75
Flammability, UL94 HB
@Thickness 1.57 mm
From Wellman QC Laboratory Testing; UL 94
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 560 - 590 °F
Middle Barrel Temperature 540 - 560 °F
Front Barrel Temperature 520 - 540 °F
Nozzle Temperature 510 - 560 °F
Melt Temperature 540 - 560 °F
Mold Temperature 160 - 200 °F
Drying Temperature 175 °FOpened bags and gaylord boxes
Dry Time 2 - 4 hourOpened bags and gaylord boxes
Moisture Content 0.050 - 0.20 %During molding to prevent hydrolytic degradation
 <= 0.20 %In shipping bags, ready to mold
Injection Pressure 5000 - 20000 psi
Back Pressure 50.0 psi
Screw Speed 30 - 120 rpm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PWEL46 / 72326

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.