MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Momentive Performance Materials GE Silicones SilPruf SCS2000 Silicone Sealant & Adhesive
Categories: Polymer; Adhesive; Thermoset; Silicone

Material Notes: GE SCS2000 is a one-component, high-strength, neutral cure silicone sealant & adhesive for use in structural glazing and on a wide variety of materials in new or remedial weatherproofing applications. SCS2000 sealant is supplied as a paste and upon cure, produces a durable, formed-in-place silicone rubber joint sealant.

Features: Silicone Durability, Strength Properties, Low VOC, ±50% Movement Capacity. SCS2000 sealant is recommended for the following applications: Weatherproofing, Structural Glazing, Protective Glazing, Adhesive.

Available colors: White (SCS2002), black(SCS2003), limestone(SCS2004), medium gray(SCS2007), light gray(SCS2008), aluminum gray(SCS2009), dark gray(SCS2010), precast white(SCS2020), bronze(SCS2097), earth tone(SCS2040), red brick(SCS2041), champagne(SCS2046), sandy beige(SCS2100.0148). Custom colored is available.

Information provided by Momentive Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Volatile Organic Compounds (VOC) Content 20 g/lUncured; WPSTM C1454
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 24ASTM D2240
Tensile Strength, Ultimate 0.970 MPaASTM C1135
 2.35 MPaASTM D412
Tensile Stress at Strain 0.320 MPa
@Strain 50 %
ASTM C1184
 0.500 MPa
@Strain 100 %
ASTM C1184
Elongation, Ultimate 353 %ASTM C1135
 715 %ASTM D412
Shear Strength 0.840 MPa
@Thickness 6.35 mm
ASTM C961
Tear Strength 13.72 kg(f)/cmDie B.; ASTM D624
Peel Strength 56.6 pli
@Temperature 23.9 °C,
Time 1.81e+6 sec
50%RH; ASTM C794
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 250 °F
Minimum Service Temperature, Air -55.0 °F
 
Processing PropertiesOriginal ValueComments
Cure Time 240 - 336 hourFull cured. Most common bead sizes.
 72.0 - 96.0 hour
@Temperature 24.0 °C
1/4" deep section. 50% RH
Tack-Free Time 36.0 - 48.0 minASTM C679
Working Life 30.0 - 40.0 min
 
Descriptive Properties
AppearancePaste
Consistency / Sag0.1" maxASTM D2202
Joint Movement Capability+/- 50%ASTM C719.
Silicone Content (%)100Uncured
UV & Weathering ResistanceExcellentGE 20 yr study

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMOMEN9918 / 265728

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.