MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
Proto3000 PPSF Fused Deposition Modeling Polymer
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polyphenylsulfone (PPSU)

Material Notes: Description: PPSF/PPSU (polyphenylsulfone) material has the greatest heat and chemical resistance of all Fortus materials - ideal for aerospace, automotive and medical applications. PPSF parts manufactured on Fortus 3D Production Systems are not only mechanically superior, but also dimensionally accurate, to better predict end-product performance. Users can also sterilize PPSF via steam autoclave, EtO sterilization, plasma sterilization, chemical sterilization and radiation. PPSF gives you the ability to manufacture Real Parts™ direct from digital ? les that are ideal for conceptual modeling, functional prototyping, manufacturing tools, and end-use-parts.

Available Colors: Tan

Information provided by Proto3000 for their protoyping engineering services.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.28 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 55.0 MPaType 1, 2"/min; ASTM D638
Elongation at Break 3.0 %ASTM D638
Tensile Modulus 2068 MPaType 1, 0.125; ASTM D638
Flexural Strength 110 MPaMethod 1, 0.05"/min; ASTM D790
Flexural Modulus 2206 MPaASTM D790
Izod Impact, Notched 58.73 J/mMethod A; ASTM D256
Izod Impact, Unnotched 1.655 J/cmASTM D256
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.45
@Frequency 60 Hz
IEC 60250
Dielectric Strength 14.6 kV/mmIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 55.0 µm/m-°CASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 189 °CASTM D648
Glass Transition Temp, Tg 230 °CDAM (SSYS)
Flammability, UL94 V-0
@Thickness 3.20 mm
 
Descriptive Properties
Environmental ResistanceAntifreeze (Prestone), 50%Passed, 24 hrs @ 23°C
 Antifreeze (Prestone), 50%Passed, 24 hrs @ 100°C
 Gasoline-UnleadedPassed, 24 hrs @ 23°C
 Motor Oil 10W-40Passed, 24 hrs @ 23°C
 Motor Oil 10W-40Passed, 24 hrs @ 100°C
 Power Steering FluidPassed, 24 hrs @ 23°C
 Power Steering FluidPassed, 24 hrs @ 100°C
 Transmission FluidPassed, 24 hrs @ 23°C
 Transmission FluidPassed, 24 hrs @ 100°C
 Windshield Washer Fluid, 50%Passed, 24 hrs @ 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Stratasys® PPSF Polyphenylsulfone for 3D Printing
Stratasys® Ultem 9085 for Rapid Prototyping
Stratasys® ABSi
Stratasys® ABS-M30
Stratasys® ABS-M30i

PPROTO974 / 133177

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.