MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Eneos N640 Nitrile Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Characteristics: Acrylate modified NBR

Application: Packing, gasket, oil sheet, diaphragm

ENEOS has acquired the elastomer product lines from JSR Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.990 g/cc
Mooney Viscosity 41
@Temperature 100 °C
ML1+4, Compound (non-vulcanized)
 50
@Temperature 100 °C
ML1+4
 26
@Temperature 125 °C,
Time 64800 sec
Scorch Test, ML1, Compound (non-vulcanized)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 63
 63Compound (vulcanized)
 51
@Temperature 40.0 °C,
Time 173000 sec
Fuel Oil B, Compound (non-vulcanized)
 54
@Temperature 120 °C,
Time 252000 sec
IRM903, Compound (vulcanized)
 61
@Temperature 120 °C,
Time 252000 sec
IRM901, Compound (vulcanized)
 68
@Temperature 120 °C,
Time 252000 sec
Air heat Aging, Compound (non-vulcanized)
Tensile Strength 14.8 MPa
 14.8 MPaCompound (vulcanized)
 6.068 MPa
@Temperature 40.0 °C,
Time 173000 sec
Fuel Oil B, Compound (non-vulcanized)
 13.024 MPa
@Temperature 120 °C,
Time 252000 sec
IRM903, Compound (vulcanized)
 14.208 MPa
@Temperature 120 °C,
Time 252000 sec
IRM901, Compound (vulcanized)
 17.908 MPa
@Temperature 120 °C,
Time 252000 sec
Air heat Aging, Compound (non-vulcanized)
Elongation at Break 300 %
 300 %Compound (vulcanized)
 150 %
@Temperature 120 °C,
Time 252000 sec
Air heat Aging, Compound (non-vulcanized)
 153 %
@Temperature 40.0 °C,
Time 173000 sec
Fuel Oil B, Compound (non-vulcanized)
 207 %
@Temperature 120 °C,
Time 252000 sec
IRM901, Compound (vulcanized)
 261 %
@Temperature 120 °C,
Time 252000 sec
IRM903, Compound (vulcanized)
100% Modulus 3.60 MPaCompound (vulcanized)
Resilience 35[%], Rebound, Compound (vulcanized)
Tear Strength 39.0 kN/mCompound (vulcanized)
Compression Set 12 %
@Temperature 100 °C,
Time 252000 sec
Compound (vulcanized)
 18 %
@Temperature 120 °C,
Time 252000 sec
Compound (vulcanized)
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -26.0 °C
 
Descriptive Properties
Acrylonitrile Content (%)25
Delta;V100 (%)-1IRM901 70 hrs at 120°C, Compound (vulcanized)
 105Fuel Oil C/Ethanol 48 hrs at 40°C, Compound (non-vulcanized)
 17IRM903 70 hrs at 120°C, Compound (vulcanized)
 2Distilled Water 70 hr at 40°C, Compound (non-vulcanized)
 33Fuel Oil B 48 hrs at 40°C, Compound (non-vulcanized)
 61Fuel Oil C 48 hrs at 40°C, Compound (non-vulcanized)
Extrusion Test16080°C, 25 rpm, Die Swell %
 311 cm/min80°C, 25 rpm, Extrusion Length
 408 cc/min80°C, 25 rpm, Extrusion Volume
Flex Test2Growth 2 to 15 mm (Thousand Times)
 60Occurrence(Thousand Times)
Flow Rate95Q×104, 80°C, 100 kg, Kokahiki Flow tester
JSR Mold Curast Test 160°C, Minutes3tc(10)
 8tc(90)
Low-Temperature Torsion Test-25°Ct10
 -30°Ct100
Mill Contraction 50°C (%)59
Ozone Degradability TestA-2Dynamic 0 to 20% Elongation, 50 ppm 5 Hours at 40°C
 C-2Static 20% Elongation, 50 ppm 5 Hours at 40°C
Product formBale
Product StainSS

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PJSRC8074 / 295390

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.