MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Pressure Seal 4503 Chloroprene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 4503 is 50 durometer black colored Neoprene elastomer, it is formulated to have good low temperature flexibility. It exhibits good resistance to compression set at moderate heat.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BC 515 A14 B14 C12 EO14 EO34 F17; 5 BC 515 A14 B14 C12 EO14 EO34 F19; 6 BC 515 A14 B14 C12 EO14 EO34 F17; 2 BE 515 A14 B14 C12 EO14 EO34 F17; 3 BE 515 A14 B14 C12 EO14 EO34 F19
MIL-STD-417 SC 515 A1 B1 E3 F2
MIL-R-6855 Class 2. Type A & B, Grade 50

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.35 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 54
 47
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 52
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 53
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 54
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 57
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 57
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 65
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 65
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 1863 psi
 892.4 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 1054.46 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 1600.3 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1973 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 1976.6 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 2123.8 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 2123.8 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Elongation, Ultimate 440 %
 249.9 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 279.8 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 399.96 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 399.96 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 410.1 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 429.9 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 440 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
100% Modulus 192 psi
Tear Strength 88.0 pliDie B; Method D 624
 128 pliDie C; Method D 624
Compression Set 7.9 %
@Temperature 100 °C,
Time 79200 sec
Solid
 12.8 %
@Temperature 100 °C,
Time 79200 sec
Plied
 14.9 %
@Temperature 100 °C,
Time 252000 sec
Solid
 22.7 %
@Temperature 100 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -67.0 °F
Shrinkage -7.40 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #1
 4.3 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 10.7 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 44.7 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 54.5 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #3
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL065 / 318275

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.