MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Crastin® SK602 NC010 PBT-GF15
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: 15% Glass Reinforced Polybutylene Terephthalate

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.41 g/ccISO 1183
Melt Density 1.22 g/cc
@Temperature 250 °C
Water Absorption 0.42 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.170 %
@Thickness 2.00 mm
Sim. to ISO 62
Viscosity Number 105 cm³/gISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0040 cm/cmISO 294-4, 2577
 0.0015 cm/cm
@Treatment Temp. 80.0 °C,
Time 173000 sec
Postmolding shrinkage; ISO 294-4
Linear Mold Shrinkage, Transverse 0.011 cm/cmISO 294-4, 2577
 0.0030 cm/cm
@Treatment Temp. 80.0 °C,
Time 173000 sec
Postmolding shrinkage; ISO 294-4
Melt Flow 15 g/10 min
@Load 2.16 kg,
Temperature 250 °C
cm³/10min Volumetric; ISO 1133
 18 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 109 MPaISO 527-1/-2
Elongation at Break 3.5 %ISO 527-1/-2
Tensile Modulus 5800 MPaISO 527-1/-2
Flexural Strength 160 MPaISO 178
Flexural Modulus 5200 MPaISO 178
Poissons Ratio 0.35
Shear Strength 50.0 MPaASTM D 732
Izod Impact, Notched (ISO) 6.00 kJ/m²
@Temperature -40.0 °C
ISO 180/1A
 6.00 kJ/m²
@Temperature -30.0 °C
ISO 180/1A
 6.50 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Izod Impact, Unnotched (ISO) 30.0 kJ/m²
@Temperature -40.0 °C
ISO 180/1U
 50.0 kJ/m²
@Temperature -30.0 °C
ISO 180/1U
 50.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1U
Charpy Impact Unnotched 40.0 kJ/m²
@Temperature -40.0 °C
ISO 179/1eU
 45.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 45.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 7.00 kJ/m²
@Temperature -40.0 °C
ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 7.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
Tensile Creep Modulus, 1 hour 5300 MPa1h; ISO 899-1
Tensile Creep Modulus, 1000 hours 4300 MPa1000h; ISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+15 ohmIEC 62631-3-2
Dielectric Constant 3.5
@Frequency 1e+6 Hz
IEC 62631-2-1
 3.8
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 27.0 kV/mmIEC 60243-1
Dissipation Factor 0.00070
@Frequency 100 Hz
IEC 62631-2-1
 0.020
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 350 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°CISO 11359-1/-2
Specific Heat Capacity 1.90 J/g-°C
@Temperature 250 °C
Melt
Thermal Conductivity 0.240 W/m-K
@Temperature 250 °C
Melt
Melting Point 225 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 220 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 200 °CISO 75-1/-2
Vicat Softening Point 205 °C50°C/h, 50N; ISO 306
Glass Transition Temp, Tg 55.0 °C10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 0.750 mm
IEC 60695-11-10
 HB
@Thickness 1.50 mm
IEC 60695-11-10
Flame Spread 30.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Oxygen Index 19 %ISO 4589-1/-2
Glow Wire Ignition Temperature 725 °C
@Thickness 3.00 mm
IEC 60695-2-13
 750 °C
@Thickness 0.750 mm
IEC 60695-2-13
 750 °C
@Thickness 1.00 mm
IEC 60695-2-13
 750 °C
@Thickness 1.50 mm
IEC 60695-2-13
 750 °C
@Thickness 2.00 mm
IEC 60695-2-13
 
Processing PropertiesOriginal ValueComments
Melt Temperature 250 °COptimum, Injection
 240 - 260 °CRange, Injection
Mold Temperature 80.0 °COptimum, Injection
 30.0 - 130 °CInjection
Ejection Temperature 170 °CInjection
Drying Temperature 120 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.040 %Injection
Hold Pressure >= 60.0 MPaInjection
 
Descriptive Properties
AdditivesRelease agent
Back pressureAs low as possible
Drying RecommendedyesInjection
Emission of organic compounds (µgC/g)140VDA 277
FMVSS ClassBISO 3795 (FMVSS 302)
Fogging (mg)0.1G-value (condensate); ISO 6452
Odor Class3VDA 270
Part Marking Code>PBT-GF15<ISO 11469
PolymerPBT-GF15
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPBT-GF15ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Crastin® SK605 NC010 PBT-GF30
Celanese Crastin® SK605 BK851 PBT-GF30
Celanese Crastin® LW9020 NC010 PBT+ASA-GF20
Ensinger Tecamid® 6/6 Nylon (PA66)
Celanese Crastin® SK602 BK851 PBT-GF15

PDSX5054 / 197694

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.