MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Syensqo (Solvay Specialty Polymers) Amodel® AFA-6133 V0 Z PPA, Conditioned
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA)

Material Notes: Data for conditioned samples. MatWeb has a more thorough entry for dry samples.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 166 MPa24100 psiASTM D638
Tensile Strength, Yield  63.4 MPa
@Temperature 175 °C
9200 psi
@Temperature 347 °F
ISO 527-2
 75.2 MPa
@Temperature 150 °C
10900 psi
@Temperature 302 °F
ISO 527-2
 114 MPa
@Temperature 100 °C
16500 psi
@Temperature 212 °F
ISO 527-2
 186 MPa
@Temperature 23.0 °C
27000 psi
@Temperature 73.4 °F
ISO 527-2
Elongation at Break 1.7 %1.7 %ASTM D638
 1.6 %
@Temperature 23.0 °C
1.6 %
@Temperature 73.4 °F
ISO 527-2
 2.4 %
@Temperature 100 °C
2.4 %
@Temperature 212 °F
ISO 527-2
 4.9 %
@Temperature 175 °C
4.9 %
@Temperature 347 °F
ISO 527-2
 5.1 %
@Temperature 150 °C
5.1 %
@Temperature 302 °F
ISO 527-2
Tensile Modulus 13.7 GPa1990 ksiASTM D638
 5.10 GPa
@Temperature 175 °C
740 ksi
@Temperature 347 °F
ISO 527-2
 5.90 GPa
@Temperature 150 °C
856 ksi
@Temperature 302 °F
ISO 527-2
 9.20 GPa
@Temperature 100 °C
1330 ksi
@Temperature 212 °F
ISO 527-2
 14.5 GPa
@Temperature 23.0 °C
2100 ksi
@Temperature 73.4 °F
ISO 527-2
Flexural Strength 229 MPa33200 psiASTM D790
 88.0 MPa
@Temperature 175 °C
12800 psi
@Temperature 347 °F
ISO 178
 101 MPa
@Temperature 150 °C
14600 psi
@Temperature 302 °F
ISO 178
 161 MPa
@Temperature 100 °C
23400 psi
@Temperature 212 °F
ISO 178
 259 MPa
@Temperature 23.0 °C
37600 psi
@Temperature 73.4 °F
ISO 178
Flexural Modulus 13.3 GPa1930 ksiASTM D790
 4.60 GPa
@Temperature 175 °C
667 ksi
@Temperature 347 °F
ISO 178
 5.00 GPa
@Temperature 150 °C
725 ksi
@Temperature 302 °F
ISO 178
 8.10 GPa
@Temperature 100 °C
1170 ksi
@Temperature 212 °F
ISO 178
 12.6 GPa
@Temperature 23.0 °C
1830 ksi
@Temperature 73.4 °F
ISO 178
Shear Strength 62.1 MPa9010 psiASTM D732
Izod Impact, Notched 0.800 J/cm1.50 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 8.00 kJ/m²3.81 ft-lb/in²Type 1, Notch A; ISO 180
Izod Impact, Unnotched (ISO) 44.0 kJ/m²20.9 ft-lb/in²Type 1; ISO 180
Charpy Impact Unnotched 4.70 J/cm²22.4 ft-lb/in²Type 1, Edgewise; ISO 179
Charpy Impact, Notched 1.40 J/cm²6.66 ft-lb/in²Type 2, Edgewise, Notch A; ISO 179
 
Thermal PropertiesMetricEnglishComments
Melting Point 310 °C590 °FISO 11357-3
Deflection Temperature at 1.8 MPa (264 psi) 282 °C540 °FUnannealed, Flatwise; ISO 75-2/A
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4078 / 279878

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.