MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
SABIC Ultem 1010RV PEI  (discontinued **)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: Enhanced flow Polyetherimide (Tg 217C) with internal mold release. ECO Conforming, UL94 V0 and 5VA listing; color dependant, see UL Yellow Card.

This data was supplied by SABIC-IP for the Americas region.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.27 g/ccASTM D 792
Density 1.27 g/ccISO 1183
Moisture Absorption at Equilibrium 0.70 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 1.25 %
@Temperature 23.0 °C
ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC Method
Melt Flow 17.8 g/10 min
@Load 6.60 kg,
Temperature 337 °C
ASTM D 1238
 25 g/10 min
@Load 5.00 kg,
Temperature 220 °C
[cm^3/10 min] Melt Volume Rate; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 85.0 MPa5 mm/min; ISO 527
 105 MPaType I, 5 mm/min; ASTM D 638
Tensile Strength, Yield 105 MPa5 mm/min; ISO 527
 110 MPaType I, 5 mm/min; ASTM D 638
Elongation at Break 60 %Type I, 5 mm/min; ASTM D 638
 60 %5 mm/min; ISO 527
Elongation at Yield 6.0 %5 mm/min; ISO 527
 7.0 %Type I, 5 mm/min; ASTM D 638
Tensile Modulus 3200 MPa1 mm/min; ISO 527
 3580 MPa5 mm/min; ASTM D 638
Flexural Yield Strength 160 MPa2 mm/min; ISO 178
 174 MPa1.3 mm/min, 50 mm span; ASTM D 790
Flexural Modulus 3300 MPa2 mm/min; ISO 178
 3420 MPa1.3 mm/min, 50 mm span; ASTM D 790
Izod Impact, Notched 32.0 J/m
@Temperature 23.0 °C
ASTM D 256
 35.0 J/m
@Temperature -30.0 °C
ASTM D 256
Izod Impact, Unnotched 13.35 J/cm
@Temperature 23.0 °C
ASTM D 4812
Izod Impact, Notched (ISO) 5.00 kJ/m²
@Temperature 23.0 °C
80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 3.00 kJ/m²
@Temperature 23.0 °C
V-notch Edgew 80*10*4 sp=62mm; ISO 179/1eA
Instrumented Impact Total Energy 33.0 J
@Temperature 23.0 °C
ASTM D 3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+17 ohm-cmASTM D 257
Dielectric Constant 3.15
@Frequency 1000 Hz
ASTM D 150
Dielectric Strength 27.9 kV/mm
@Thickness 1.60 mm
in oil; ASTM D 149
 32.6 kV/mm
@Thickness 1.60 mm
in air; ASTM D 149
Dissipation Factor 0.0013
@Frequency 1000 Hz
ASTM D 150
 0.0025
@Frequency 2.45e+9 Hz
ASTM D 150
Arc Resistance 120 - 180 secTungsten, PLC code 5; ASTM D 495
Comparative Tracking Index 100 - 175 VPLC code 4; UL 746A
Hot Wire Ignition, HWI 60 - 120 secPLC code 1; UL 746A
High Amp Arc Ignition, HAI 15 - 30 arcssurface, PLC code 3; UL 746A
High Voltage Arc-Tracking Rate, HVTR 25.4 - 80.0 mm/minPLC code 2; UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 55.8 µm/m-°C
@Temperature -20.0 - 150 °C
ASTM E 831
CTE, linear, Transverse to Flow 50.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
 50.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Thermal Conductivity 0.220 W/m-KASTM C 177
Deflection Temperature at 1.8 MPa (264 psi) 193 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 198 °C
@Thickness 6.40 mm
unannealed; ASTM D 648
Vicat Softening Point 211 °CRate B/50; ISO 306
 212 °CRate B/120; ISO 306
 218 °CRate B/50; ASTM D 1525
Glass Transition Temp, Tg 217 °C
UL RTI, Electrical 170 °CUL 746B
UL RTI, Mechanical with Impact 170 °CUL 746B
UL RTI, Mechanical without Impact 170 °CUL 746B
Flammability, UL94 V-1
@Thickness 0.750 mm
UL 94
 V-0
@Thickness 0.750 mm
UL 94
 5VA
@Thickness 3.00 mm
UL 94
Smoke Density 2.0
@Time 240 sec
NBS, Flaming, Ds; ASTM E 662
Oxygen Index 44 %LOI; ASTM D 2863

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABIC2913 / 116801

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.