Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.22 g/cc | 1.22 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 91 | 91 |
| 77 @Treatment Temp. 23.0 °C, Time 252000 sec | 77 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 79 @Treatment Temp. 23.0 °C, Time 252000 sec | 79 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 87 @Treatment Temp. 100 °C, Time 252000 sec | 87 @Treatment Temp. 212 °F, Time 70.0 hour |
| 87 @Treatment Temp. 125 °C, Time 252000 sec | 87 @Treatment Temp. 257 °F, Time 70.0 hour |
| 87 @Treatment Temp. 150 °C, Time 252000 sec | 87 @Treatment Temp. 302 °F, Time 70.0 hour |
| 90 @Treatment Temp. 23.0 °C, Time 252000 sec | 90 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 90 @Treatment Temp. 100 °C, Time 252000 sec | 90 @Treatment Temp. 212 °F, Time 70.0 hour |
| 91 @Treatment Temp. 100 °C, Time 252000 sec | 91 @Treatment Temp. 212 °F, Time 70.0 hour |
| 92 @Treatment Temp. 125 °C, Time 252000 sec | 92 @Treatment Temp. 257 °F, Time 70.0 hour |
| 92 @Treatment Temp. 150 °C, Time 252000 sec | 92 @Treatment Temp. 302 °F, Time 70.0 hour |
| 93 @Treatment Temp. 100 °C, Time 252000 sec | 93 @Treatment Temp. 212 °F, Time 70.0 hour |
| 93 @Treatment Temp. 125 °C, Time 252000 sec | 93 @Treatment Temp. 257 °F, Time 70.0 hour |
| 93 @Treatment Temp. 100 °C, Time 252000 sec | 93 @Treatment Temp. 212 °F, Time 70.0 hour |
| 95 @Treatment Temp. 150 °C, Time 252000 sec | 95 @Treatment Temp. 302 °F, Time 70.0 hour |
Tensile Strength | 21.42 MPa | 3107 psi |
| 12.832 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1861.1 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 14.181 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 2056.8 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 19.8154 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 2873.98 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 20.586 MPa @Treatment Temp. 125 °C, Time 252000 sec | 2985.8 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 20.630 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2992.1 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 20.886 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3029.3 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 20.886 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3029.3 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 21.958 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3184.7 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 22.536 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3268.6 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 22.943 MPa @Treatment Temp. 150 °C, Time 252000 sec | 3327.6 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 23.093 MPa @Treatment Temp. 125 °C, Time 252000 sec | 3349.3 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 23.1143 MPa @Treatment Temp. 125 °C, Time 252000 sec | 3352.45 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 23.715 MPa @Treatment Temp. 150 °C, Time 252000 sec | 3439.5 psi @Treatment Temp. 302 °F, Time 70.0 hour |
Elongation, Ultimate | 158 % | 158 % |
| 94.6 % @Treatment Temp. 23.0 °C, Time 252000 sec | 94.6 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 107 % @Treatment Temp. 23.0 °C, Time 252000 sec | 107 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 121.1 % @Treatment Temp. 125 °C, Time 252000 sec | 121.1 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 121.66 % @Treatment Temp. 150 °C, Time 252000 sec | 121.66 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 134 % @Treatment Temp. 100 °C, Time 252000 sec | 134 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 139.99 % @Treatment Temp. 100 °C, Time 252000 sec | 139.99 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 149 % @Treatment Temp. 23.0 °C, Time 252000 sec | 149 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 149.8 % @Treatment Temp. 100 °C, Time 252000 sec | 149.8 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 152.3 % @Treatment Temp. 150 °C, Time 252000 sec | 152.3 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 154.05 % @Treatment Temp. 100 °C, Time 252000 sec | 154.05 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 170.3 % @Treatment Temp. 125 °C, Time 252000 sec | 170.3 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 170.5 % @Treatment Temp. 125 °C, Time 252000 sec | 170.5 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 174.9 % @Treatment Temp. 150 °C, Time 252000 sec | 174.9 % @Treatment Temp. 302 °F, Time 70.0 hour |
50% Modulus | 8.074 MPa | 8.074 MPa |
100% Modulus | 16.24 MPa | 2355 psi |
Tear Strength | 37.7 kN/m | 215 pli |
| 42.4 kN/m | 242 pli |
Compression Set | 8.4 % @Treatment Temp. 100 °C, Time 79200 sec | 8.4 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 9.1 % @Treatment Temp. 125 °C, Time 79200 sec | 9.1 % @Treatment Temp. 257 °F, Time 22.0 hour |
| 11.4 % @Treatment Temp. 100 °C, Time 252000 sec | 11.4 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 13 % @Treatment Temp. 100 °C, Time 79200 sec | 13 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 14 % @Treatment Temp. 125 °C, Time 79200 sec | 14 % @Treatment Temp. 257 °F, Time 22.0 hour |
| 14 % @Treatment Temp. 100 °C, Time 252000 sec | 14 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 17 % @Treatment Temp. 150 °C, Time 79200 sec | 17 % @Treatment Temp. 302 °F, Time 22.0 hour |
| 31.2 % @Treatment Temp. 150 °C, Time 79200 sec | 31.2 % @Treatment Temp. 302 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -37.2 °C | -35.0 °F |
Shrinkage | -2.10 % @Treatment Temp. 125 °C, Time 252000 sec | -2.10 % @Treatment Temp. 257 °F, Time 70.0 hour |
| -2.10 % @Treatment Temp. 150 °C, Time 252000 sec | -2.10 % @Treatment Temp. 302 °F, Time 70.0 hour |
| -2.00 % @Treatment Temp. 100 °C, Time 252000 sec | -2.00 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 1.2 % @Treatment Temp. 23.0 °C, Time 252000 sec | 1.2 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 1.4 % @Treatment Temp. 100 °C, Time 252000 sec | 1.4 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 8.9 % @Treatment Temp. 100 °C, Time 252000 sec | 8.9 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 9.3 % @Treatment Temp. 125 °C, Time 252000 sec | 9.3 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 10.3 % @Treatment Temp. 150 °C, Time 252000 sec | 10.3 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 28.6 % @Treatment Temp. 23.0 °C, Time 252000 sec | 28.6 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 46 % @Treatment Temp. 23.0 °C, Time 252000 sec | 46 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |
TR-10 Temperature | -29°C |