MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Chemours Viton® A-200 with 2 phr VC50 Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Lower viscosity
  • Improved mold flow
  • Excellent extrusion characteristics
  • Better mold release
  • Less mold fouling
  • Improved compression set resistance

Applications

  • Transfer and injection molding for O-rings, Valve stem seals and shaft seals, and Parts with complicated shapes
  • Extrusions for Fuel hose and tubing
  • Solution coating for Fabric and Tanks or chemical containers

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 666624 hours Postcure; ASTM D2240
Tensile Strength at Break 12.1 MPa1750 psi24 hours Postcure; ASTM D412
Elongation at Break 250 %250 %24 hours Post cure; ASTM D412
100% Modulus 3.60 MPa
@Strain 100 %
522 psi
@Strain 100 %
24 hours Postcure; ASTM D412
Compression Set  12 %
@Temperature 23.0 °C,
Time 252000 sec
12 %
@Temperature 73.4 °F,
Time 70.0 hour
O-Rings; ASTM D395B
 12 %
@Temperature 200 °C,
Time 252000 sec
12 %
@Temperature 392 °F,
Time 70.0 hour
O-Rings; ASTM D395B
 15 %
@Temperature 232 °C,
Time 79200 sec
15 %
@Temperature 450 °F,
Time 22.0 hour
O-Rings; ASTM D395B
 26 %
@Temperature 200 °C,
Time 1.21e+6 sec
26 %
@Temperature 392 °F,
Time 336 hour
O-Rings; ASTM D395B
 
Processing PropertiesMetricEnglishComments
Processing Temperature  180 °C
@Time 601 sec
356 °F
@Time 0.167 hour
Press Cure
 232 °C
@Time 86400 sec
450 °F
@Time 24.0 hour
Postcure
 
Descriptive Properties
Formulation as Tested2Viton® Curative #50
 20MT Black
 3MgO
 6Ca(OH)2
 98A-200

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chemours Viton® A-200 with 45 MT Black and 2.5 VC50 Fluoroelastomer Compound
Chemours Viton® A-200 with 30 MT Black and 2.5 VC50 Fluoroelastomer Compound
Chemours Viton® A-200 with 2.5phr VC50 Fluoroelastomer Compound
Chemours Viton® A-200 with 2 MT Black and 2.5 VC50 Fluoroelastomer Compound
Chemours Viton® A-200 with 2 MT Black and 1.5 VC50 Fluoroelastomer Compound

PDVC9882 / 170523

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.