MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Lehvoss LUVOCOM® 1100/GF/20/EM/MR/L Polyethersulfone, 20% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyethersulfone (PES); Polyethersulfone (PES), 10%Glass Fiber Filled

Material Notes: Polyethersulfone with glass fibers, easy flowing, demolding aid, natural color (beige)

Main features: High dimensionally stable precision parts, even at elevated temperatures and narrow tolerance range. Especially suitable for thin wall complex parts. Suitable for parts in contact with drinking water.

Information provided by Lehmann & Voss & Co.KG

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.51 g/cc1.51 g/ccISO 1183-3
Water Absorption <= 0.100 %
@Time 86400 sec
<= 0.100 %
@Time 24.0 hour
ISO 62
Linear Mold Shrinkage 0.00300 - 0.00500 cm/cm0.00300 - 0.00500 in/inDIN 16742
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 135 MPa19600 psi50 mm/min; ISO 527
Elongation at Break 2.40 %2.40 %50 mm/min, Fmax; ISO 527
Tensile Modulus 8.00 GPa1160 ksi1 mm/min; ISO 527
Flexural Strength 150 MPa21800 psi10 mm/min; ISO 178
Flexural Modulus 6.00 GPa870 ksi2 mm/min; ISO 178
Flexural Strain at Break 3.80 %3.80 %10 mm/min, Fmax; ISO 178
Charpy Impact Unnotched 4.00 J/cm²19.0 ft-lb/in²80x10x4mm; ISO 179 1eU
Charpy Impact, Notched 1.00 J/cm²4.76 ft-lb/in²80x10x4mm; ISO 179 1eA
 
Electrical PropertiesMetricEnglishComments
Insulation Resistance <= 1.00e+12 ohm<= 1.00e+12 ohmstrip electrode R25; DIN EN 62631-3-3
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 31.0 µm/m-°C17.2 µin/in-°F10x8x4 mm; ISO 11359
Maximum Service Temperature, Air  180 °C
@Time 7.20e+7 sec
356 °F
@Time 20000 hour
Continuous; IEC 60216
 200 °C
@Time 720000 sec
392 °F
@Time 200 hour
during lifetime
Deflection Temperature at 1.8 MPa (264 psi) 210 °C410 °F80x10x4mm; ISO 75
Vicat Softening Point 220 °C428 °FVST A; DIN ISO 306
Flammability, UL94 V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 340 - 360 °C644 - 680 °F
Zone 1 355 - 375 °C671 - 707 °F
Zone 2 360 - 380 °C680 - 716 °F
Zone 3 350 - 370 °C662 - 698 °F
Melt Temperature 350 °C662 °F
Mold Temperature 120 - 200 °C248 - 392 °F
Drying Temperature 150 °C
@Time 10800 - 18000 sec
302 °F
@Time 3.00 - 5.00 hour
Dehumidifying

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PLUU8709 / 325093

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.