MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Celanese Zytel® HTN54G35EF BK420 PA-IGF35
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 40% Glass Fiber Reinforced

Material Notes: 35% Glass Reinforced, Toughened, PPA, High Performance Polyamide Developed for Electrical and Electronics Applications

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.42 g/cc0.0513 lb/in³DAM; ISO 1183
Moisture Absorption 1.80 %
@Thickness 2.00 mm
1.80 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Viscosity Number 120 cm³/g1.20 dl/gDAM; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0050 cm/cm0.0050 in/inDAM; ISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 190 MPa27600 psiDAM; ISO 527-1/-2
Elongation at Break 3.0 %3.0 %DAM; ISO 527-1/-2
Tensile Modulus 11.0 GPa1600 ksiDAM; ISO 527-1/-2
Flexural Strength 270 MPa39200 psiDAM; ISO 178
Flexural Modulus 10.0 GPa1450 ksiDAM; ISO 178
Poissons Ratio 0.340.34DAM
Charpy Impact Unnotched 8.20 J/cm²
@Temperature 23.0 °C
39.0 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
Charpy Impact, Notched 1.10 J/cm²
@Temperature 23.0 °C
5.23 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmDAM; IEC 62631-3-1
Dielectric Constant  3.9
@Frequency 1e+6 Hz
3.9
@Frequency 1e+6 Hz
DAM; IEC 62631-2-1
 4.3
@Frequency 100 Hz
4.3
@Frequency 100 Hz
DAM; IEC 62631-2-1
Dielectric Strength 31.0 kV/mm787 kV/in50% RH; IEC 60243-1
 32.0 kV/mm813 kV/inDAM; IEC 60243-1
Dissipation Factor  0.0050
@Frequency 100 Hz
0.0050
@Frequency 100 Hz
DAM; IEC 62631-2-1
 0.0155
@Frequency 1e+6 Hz
0.0155
@Frequency 1e+6 Hz
DAM; IEC 62631-2-1
Comparative Tracking Index 600 V600 VDAM; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C11.1 µin/in-°FDAM; ISO 11359-1/-2
 19.0 µm/m-°C
@Temperature 55.0 - 160 °C
10.6 µin/in-°F
@Temperature 131 - 320 °F
DAM; ISO 11359-1/-2
 20.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
11.1 µin/in-°F
@Temperature -40.0 - 73.4 °F
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 60.0 µm/m-°C33.3 µin/in-°FDAM; ISO 11359-1/-2
 55.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
30.6 µin/in-°F
@Temperature -40.0 - 73.4 °F
DAM; ISO 11359-1/-2
 108 µm/m-°C
@Temperature 55.0 - 160 °C
60.0 µin/in-°F
@Temperature 131 - 320 °F
DAM; ISO 11359-1/-2
Melting Point 300 °C572 °Ffirst heat; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 262 °C504 °FDAM; ISO 75-1/-2
Glass Transition Temp, Tg 65.0 °C149 °F10°C/min; 50% RH; ISO 11357-1/-2
 115 °C239 °F10°C/min; DAM; ISO 11357-1/-2
Oxygen Index 23 %23 %DAM; ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 325 °C617 °FOptimum, Injection
 320 - 330 °C608 - 626 °FRange, Injection
Mold Temperature 90.0 - 130 °C194 - 266 °FInjection
Drying Temperature 100 °C212 °FInjection
Dry Time 6.00 - 8.00 hour6.00 - 8.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.10 %<= 0.10 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
FMVSS ClassSEISO 3795 (FMVSS 302)
ISO designationISO 16396-PA-I,GF35,M1CGHR,S12-110
Part Marking Code>PA-IGF35<ISO 11469
 >PPA-IGF35<SAE J1344
PolymerPA*-I-GF35
Resin IdentificationPA-IGF35ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDSX5442f / 291022

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.