Physical Properties | Metric | English | Comments |
---|
Mooney Viscosity | 75 @Temperature 100 °C | 75 @Temperature 212 °F |
| 79 @Temperature 100 °C | 79 @Temperature 212 °F |
| 48 @Temperature 125 °C, Time 68400 sec | 48 @Temperature 257 °F, Time 19.0 hour |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 70 | 70 |
| 70 | 70 |
| 58 @Temperature 40.0 °C, Time 173000 sec | 58 @Temperature 104 °F, Time 48.0 hour |
| 67 @Temperature 120 °C, Time 252000 sec | 67 @Temperature 248 °F, Time 70.0 hour |
| 74 @Temperature 120 °C, Time 252000 sec | 74 @Temperature 248 °F, Time 70.0 hour |
| 77 @Temperature 120 °C, Time 252000 sec | 77 @Temperature 248 °F, Time 70.0 hour |
Tensile Strength | 21.6 MPa | 3130 psi |
| 21.6 MPa | 3130 psi |
| 10.368 MPa @Temperature 40.0 °C, Time 173000 sec | 1503.8 psi @Temperature 104 °F, Time 48.0 hour |
| 20.952 MPa @Temperature 120 °C, Time 252000 sec | 3038.8 psi @Temperature 248 °F, Time 70.0 hour |
| 21.168 MPa @Temperature 120 °C, Time 252000 sec | 3070.2 psi @Temperature 248 °F, Time 70.0 hour |
| 22.896 MPa @Temperature 120 °C, Time 252000 sec | 3320.8 psi @Temperature 248 °F, Time 70.0 hour |
Elongation at Break | 460 % | 460 % |
| 460 % | 460 % |
| 257.6 % @Temperature 40.0 °C, Time 173000 sec | 257.6 % @Temperature 104 °F, Time 48.0 hour |
| 287.4 % @Temperature 120 °C, Time 252000 sec | 287.4 % @Temperature 248 °F, Time 70.0 hour |
| 317.4 % @Temperature 120 °C, Time 252000 sec | 317.4 % @Temperature 248 °F, Time 70.0 hour |
| 372.6 % @Temperature 120 °C, Time 252000 sec | 372.6 % @Temperature 248 °F, Time 70.0 hour |
100% Modulus | 3.30 MPa | 479 psi |
300% Modulus | 16.3 MPa | 2360 psi |
| 16.3 MPa | 2360 psi |
Resilience | 21 | 21 |
Tear Strength | 53.0 kN/m | 302 pli |
Compression Set | 13 % @Temperature 100 °C, Time 252000 sec | 13 % @Temperature 212 °F, Time 70.0 hour |
| 19 % @Temperature 120 °C, Time 252000 sec | 19 % @Temperature 248 °F, Time 70.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -17.0 °C | 1.40 °F |
|
Descriptive Properties |
---|
Acrylonitrile Content (%) | 41.5 |
Delta;V100 (%) | 2 |
| -2 |
| 23 |
| 39 |
| 60 |
| 9 |
Extrusion Test | 115 |
| 415 cm/min |
| 440 cc/min |
Flex Test | 24 |
| 5 |
Flow Rate | 13 |
JSR Mold Curast Test 160°C, Minutes | 3 |
| 6 |
Low-Temperature Torsion Test | -15°C |
| -22°C |
Mill Contraction 50°C (%) | 39 |
Ozone Degradability Test | C-3 |
| C-3 |
Product form | Bale |
Product Stain | SS |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.