Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.87 g/cc | 1.87 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 73 | 73 |
| 63 @Treatment Temp. 200 °C, Time 252000 sec | 63 @Treatment Temp. 392 °F, Time 70.0 hour |
| 68 @Treatment Temp. 200 °C, Time 252000 sec | 68 @Treatment Temp. 392 °F, Time 70.0 hour |
| 70 @Treatment Temp. 23.0 °C, Time 252000 sec | 70 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 71 @Treatment Temp. 150 °C, Time 252000 sec | 71 @Treatment Temp. 302 °F, Time 70.0 hour |
| 73 @Treatment Temp. 150 °C, Time 252000 sec | 73 @Treatment Temp. 302 °F, Time 70.0 hour |
| 73 @Treatment Temp. 100 °C, Time 252000 sec | 73 @Treatment Temp. 212 °F, Time 70.0 hour |
| 73 @Treatment Temp. 23.0 °C, Time 252000 sec | 73 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 75 @Treatment Temp. 250 °C, Time 252000 sec | 75 @Treatment Temp. 482 °F, Time 70.0 hour |
| 78 @Treatment Temp. 275 °C, Time 252000 sec | 78 @Treatment Temp. 527 °F, Time 70.0 hour |
Tensile Strength | 10.5 MPa | 1520 psi |
| 8.5729 MPa @Treatment Temp. 200 °C, Time 252000 sec | 1243.4 psi @Treatment Temp. 392 °F, Time 70.0 hour |
| 8.8239 MPa @Treatment Temp. 275 °C, Time 252000 sec | 1279.8 psi @Treatment Temp. 527 °F, Time 70.0 hour |
| 9.2541 MPa @Treatment Temp. 200 °C, Time 252000 sec | 1342.2 psi @Treatment Temp. 392 °F, Time 70.0 hour |
| 9.6313 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1396.9 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 10.344 MPa @Treatment Temp. 150 °C, Time 252000 sec | 1500.2 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 10.679 MPa @Treatment Temp. 150 °C, Time 252000 sec | 1548.9 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 10.690 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1550.4 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 10.815 MPa @Treatment Temp. 250 °C, Time 252000 sec | 1568.6 psi @Treatment Temp. 482 °F, Time 70.0 hour |
Elongation, Ultimate | 260 % | 260 % |
| 250.1 % @Treatment Temp. 250 °C, Time 252000 sec | 250.1 % @Treatment Temp. 482 °F, Time 70.0 hour |
| 250.11 % @Treatment Temp. 150 °C, Time 252000 sec | 250.11 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 259.9 % @Treatment Temp. 150 °C, Time 252000 sec | 259.9 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 260 % @Treatment Temp. 23.0 °C, Time 252000 sec | 260 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 269.9 % @Treatment Temp. 200 °C, Time 252000 sec | 269.9 % @Treatment Temp. 392 °F, Time 70.0 hour |
| 269.9 % @Treatment Temp. 275 °C, Time 252000 sec | 269.9 % @Treatment Temp. 527 °F, Time 70.0 hour |
| 280 % @Treatment Temp. 23.0 °C, Time 252000 sec | 280 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 289.6 % @Treatment Temp. 200 °C, Time 252000 sec | 289.6 % @Treatment Temp. 392 °F, Time 70.0 hour |
100% Modulus | 4.54 MPa | 658 psi |
Tear Strength | 25.6 kN/m | 146 pli |
Compression Set | 10.5 % @Treatment Temp. 175 °C, Time 79200 sec | 10.5 % @Treatment Temp. 347 °F, Time 22.0 hour |
| 14.7 % @Treatment Temp. 23.0 °C, Time 79200 sec | 14.7 % @Treatment Temp. 73.4 °F, Time 22.0 hour |
| 14.9 % @Treatment Temp. 200 °C, Time 79200 sec | 14.9 % @Treatment Temp. 392 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -13.9 °C | 7.00 °F |
Shrinkage | 0.30 % @Treatment Temp. 23.0 °C, Time 252000 sec | 0.30 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 0.30 % @Treatment Temp. 150 °C, Time 252000 sec | 0.30 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 1.2 % @Treatment Temp. 150 °C, Time 252000 sec | 1.2 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 3.3 % @Treatment Temp. 100 °C, Time 252000 sec | 3.3 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 4.4 % @Treatment Temp. 23.0 °C, Time 252000 sec | 4.4 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 8.7 % @Treatment Temp. 200 °C, Time 252000 sec | 8.7 % @Treatment Temp. 392 °F, Time 70.0 hour |
| 15.7 % @Treatment Temp. 200 °C, Time 252000 sec | 15.7 % @Treatment Temp. 392 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |