MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Nickel silver 65-15, UNS C75400
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Excellent corrosion resistance. Fabricated by blanking, drawing, etching, forming and bending, heading and upsetting, roll threading and knurling, shearing, spinning, squeezing, stamping and swaging.

Applications: camera parts, optical equipment, etching stock, jewelry.

Available as flat products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.70 g/cc0.314 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 365 - 634 MPa52900 - 92000 psi
Tensile Strength, Yield 124 - 545 MPa18000 - 79000 psiDepending on temper
Elongation at Break 43 %43 %in 50.8 mm.
Modulus of Elasticity 125 GPa18100 ksi
Poissons Ratio 0.330.33Calculated
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 47.0 GPa6820 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 16.2 µm/m-°C
@Temperature 20.0 - 300 °C
9.00 µin/in-°F
@Temperature 68.0 - 572 °F
Thermal Conductivity 36.0 W/m-K
@Temperature 20.0 °C
250 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1040 - 1075 °C1900 - 1967 °F
Solidus 1040 °C1900 °F
Liquidus 1075 °C1967 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 63.5 - 66.5 %63.5 - 66.5 %
Iron, Fe <= 0.25 %<= 0.25 %
Lead, Pb <= 0.10 %<= 0.10 %
Manganese, Mn <= 0.50 %<= 0.50 %
Nickel, Ni 14 - 16 %14 - 16 %
Other, total <= 0.50 %<= 0.50 %
Zinc, Zn 20 %20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tin-Bearing Copper Nickel, UNS C72500, Quarter Hard flat products
Nickel silver 65-10, UNS C74500
Nickel silver 65-10, UNS C74500, OSO70 Temper flat products
Nickel silver 65-18, UNS C75200, OSO35 Temper rod
Copper Nickel Tin, UNS C72800

MC75400b1 / 11808

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.