MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Domo TECHNYL® A 30 H1 V30 PA66, 30% glass fiber, DRY
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Description: TECHNYL® A 30H1 V30 is a brominated flame retardant polyamide 66, reinforced with 30% of glass fiber, for injection molding. This product is available in natural & black color.

Benefits: This product offers excellent flame retardancy properties (UL 94, GWIT) combined with excellent processing, mechanical and electrical performance.

Available in: Asia Pacific, Europe, Latin America and North America

Regulations compliance: Grades produced or imported in Europe comply with directive 453/2010/EC, which amends REACH directive 1907/2006/EC. This grade complies with RoHS directive 2002/95/EC. Unless specified, this grade is not suitable for food contact, medical devices or toy applications.

Applications: This product is ideally suited for appliance and industrial control applications such as switches, timers and contactors.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.57 g/ccISO 1183/A
Water Absorption 0.80 %
@Temperature 23.0 °C,
Time 86400 sec
ISO 62
Viscosity 70 cP
@Shear Rate 100 1/s,
Temperature 300 °C
 105 cP
@Shear Rate 100 1/s,
Temperature 290 °C
 120 cP
@Shear Rate 100 1/s,
Temperature 280 °C
Linear Mold Shrinkage 0.0063 cm/cmIsotropy
Linear Mold Shrinkage, Flow 0.0060 cm/cm
Linear Mold Shrinkage, Transverse 0.0095 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 130 MPaISO 527 Type 1A
 140 MPaASTM D638
Tensile Stress at Strain 45.0 MPa
@Strain 0.5 %
 75.0 MPa
@Strain 1.5 %
 80.0 MPa
@Strain 1 %
Elongation at Break 2.2 %ISO 527 Type 1A
 2.5 %ASTM D638
Tensile Modulus 10000 MPaISO 527 Type 1A
Flexural Strength 200 MPaISO 178
 200 MPaASTM D790
Flexural Modulus 9500 MPaISO 178
 9500 MPaASTM D790
Izod Impact, Notched 115 J/mASTM D256
Izod Impact, Notched (ISO) 10.0 kJ/m²ISO 180/1eA
Charpy Impact Unnotched 42.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 9.50 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+14 ohmIEC 60093
Dielectric Constant 3.3IEC 60250
Dielectric Strength 42.0 kV/mmIEC 60243
Dissipation Factor 0.010IEC 60250
Comparative Tracking Index 400 VSolution B; IEC 60112
 450 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 263 °CISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 226 °CISO 75/Af
UL RTI, Electrical 130 °C
@Thickness 0.750 mm
 130 °C
@Thickness 1.50 mm
 130 °C
@Thickness 3.00 mm
UL RTI, Mechanical with Impact 90.0 °C
@Thickness 0.750 mm
 100 °C
@Thickness 1.50 mm
 100 °C
@Thickness 3.00 mm
Flammability, UL94 V-0
@Thickness 0.800 mm
1210
 V-0
@Thickness 1.60 mm
1210
 V-0
@Thickness 3.20 mm
1210
Oxygen Index 31 %ISO 4589
Glow Wire Ignition Temperature 800 °C
@Thickness 0.800 mm
ISO 60695-2-13
 825 °C
@Thickness 1.60 mm
ISO 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.800 mm
ISO 60695-2-12
 960 °C
@Thickness 1.60 mm
ISO 60695-2-12
 960 °C
@Thickness 3.20 mm
ISO 60695-2-12
 
Processing PropertiesOriginal ValueComments
Feed Temperature 270 - 280 °C
Mold Temperature 70.0 - 100 °C
Drying Temperature 80.0 °C
Moisture Content <= 0.20 %
 
Descriptive Properties
Compression Zone275-285°C
Fire and smoke F indexI3/F3NF F 16 101
Mixing Zone280-290°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Domo TECHNYL® A 30 H1 V30 PA66, 30% glass fiber, Conditioned
EMS-Grivory Grilamid® 2D 20 nat PA612
Avient Lubri-Tech™ NN-30GF/15T HS FR Nylon 6/6, Glass Filled
Domo TECHNYL® A 218 PA66, 33% glass fiber, DRY
Azoty Tarnow™ Tarnamid® T-27 MCS V0 Polyamide 6 - Flame Retarded, Unreinforced

PRHOD706 / 137937

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.