MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
SEKISUI SPI KYDEX® 2210LT Thermoplastic sheet
Categories: Polymer; Thermoplastic

Material Notes: KYDEX® 2210LT is a high performance thermoplastic sheet designed for use in rail interior applications where EN45545 R1 & R6 Hazard Level 2 compliance is required.

KYDEX® 2210LT is an alternative to FRP, metal and melamine that offers significant weight savings.

Suggested Application:

  • Seatbacks
  • Armrests
  • Window Shrouds
  • Bulkhead Components
  • Wall and Ceiling Panels
Features:
  • Meets the stringent requirements of EN45545, R1 & R6 Hazard Level 2 for EN45545
  • Integral color eliminates the need for painting or gel coat.
  • Excellent resistance to graffiti, chemicals, and staining
  • Excellent formability and fabrication characteristics
  • Available in P3 - Velour Matte and PC - Level Haircell textures
  • This product is only certified in thicknesses between 2mm-4.75mm

Information provided by SEKISUI KYDEX, LLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.35 g/ccASTM D792
Water Absorption 0.120 %
@Time 86400 sec
ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 116ASTM D785
Tensile Strength 64.1 MPaASTM D638
Tensile Modulus 5078 MPaASTM D638
Flexural Strength 100 MPaASTM D790
Flexural Modulus 4420 MPaASTM D790
Compressive Yield Strength 194.1 MPaASTM D695
Compressive Modulus 2775 MPaASTM D695
Bearing Yield Strength 16.9 MPa
@Strain 4.00 %
ASTM D953
Poissons Ratio 0.499ASTM D638
Shear Strength 49.3 MPaASTM D732
Izod Impact, Notched 48.6 J/mASTM D256
Gardner Impact 32.9 JDrop Dart Impact, GE; ASTM D5420
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 16.3 kV/mmASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 96.6 µm/m-°CASTM E831
CTE, linear, Transverse to Flow 87.3 µm/m-°CASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 98.9 °Cannealed; ASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSEKIS504 / 325244

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.