MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Sandvik Sanicro 25 Tube and pipe, seamless
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Sanicro 25 is an austenitic 22Cr25NiWCoCu stainless steel material with excellent high temperature properties, designed for use in advanced pulverized coal fired steam boilers. The grade is characterized by:
  • Very high creep strength
  • High oxidation resistance
  • High structural stability
  • Good fabricability

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 185
Tensile Strength, Ultimate >= 355 MPa
 >= 455 MPa
@Temperature 800 °C
 >= 500 MPa
@Temperature 700 °C
 >= 535 MPa
@Temperature 600 °C
 >= 550 MPa
@Temperature 500 °C
 >= 560 MPa
@Temperature 400 °C
 >= 575 MPa
@Temperature 300 °C
 >= 625 MPa
@Temperature 200 °C
 >= 680 MPa
@Temperature 100 °C
Tensile Strength, Yield >= 310 MPa
@Strain 0.2 %
 >= 355 MPa
@Strain 1 %
 >= 180 MPa
@Strain 0.2 %,
Temperature 600 °C
 >= 180 MPa
@Strain 0.2 %,
Temperature 700 °C
 >= 180 MPa
@Strain 0.2 %,
Temperature 800 °C
 >= 195 MPa
@Strain 1 %,
Temperature 700 °C
 >= 195 MPa
@Strain 1 %,
Temperature 800 °C
 >= 195 MPa
@Strain 0.2 %,
Temperature 500 °C
 >= 200 MPa
@Strain 0.2 %,
Temperature 400 °C
 >= 205 MPa
@Strain 1 %,
Temperature 600 °C
 >= 210 MPa
@Strain 0.2 %,
Temperature 300 °C
 >= 215 MPa
@Strain 1 %,
Temperature 500 °C
 >= 225 MPa
@Strain 1 %,
Temperature 400 °C
 >= 225 MPa
@Strain 0.2 %,
Temperature 200 °C
 >= 240 MPa
@Strain 1 %,
Temperature 300 °C
 >= 250 MPa
@Strain 0.2 %,
Temperature 100 °C
 >= 255 MPa
@Strain 1 %,
Temperature 200 °C
 >= 315 MPa
@Strain 1 %,
Temperature 100 °C
Elongation at Break >= 40 %Based on L = 5.65 vS where L is the original gauge length and S is the original cross section area.
 >= 40 %
Rupture Strength 25.0 MPa
@Temperature 800 °C,
Time 3.60e+8 sec
 50.0 MPa
@Temperature 800 °C,
Time 3.60e+7 sec
 50.0 MPa
@Temperature 750 °C,
Time 3.60e+8 sec
 85.0 MPa
@Temperature 750 °C,
Time 3.60e+7 sec
 95.0 MPa
@Temperature 700 °C,
Time 3.60e+8 sec
 145 MPa
@Temperature 700 °C,
Time 3.60e+7 sec
 155 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
 230 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
 230 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
 310 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
 325 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
 380 MPa
@Temperature 550 °C,
Time 3.60e+7 sec
 405 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
 500 MPa
@Temperature 500 °C,
Time 3.60e+7 sec
Modulus of Elasticity 137 GPa
@Temperature 800 °C
 145 GPa
@Temperature 700 °C
 153 GPa
@Temperature 600 °C
 160 GPa
@Temperature 500 °C
 168 GPa
@Temperature 400 °C
 175 GPa
@Temperature 300 °C
 183 GPa
@Temperature 200 °C
 191 GPa
@Temperature 100 °C
 197 GPa
@Temperature 20.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000980 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 14.5 µm/m-°C
@Temperature 30.0 - 100 °C
 15.0 µm/m-°C
@Temperature 30.0 - 200 °C
 16.0 µm/m-°C
@Temperature 30.0 - 300 °C
 16.0 µm/m-°C
@Temperature 30.0 - 400 °C
 16.0 µm/m-°C
@Temperature 100 - 200 °C
 16.5 µm/m-°C
@Temperature 30.0 - 500 °C
 16.5 µm/m-°C
@Temperature 30.0 - 600 °C
 16.5 µm/m-°C
@Temperature 200 - 300 °C
 16.5 µm/m-°C
@Temperature 300 - 400 °C
 17.0 µm/m-°C
@Temperature 400 - 500 °C
 17.0 µm/m-°C
@Temperature 30.0 - 700 °C
 17.0 µm/m-°C
@Temperature 30.0 - 800 °C
 17.5 µm/m-°C
@Temperature 30.0 - 900 °C
 18.0 µm/m-°C
@Temperature 30.0 - 1000 °C
 18.0 µm/m-°C
@Temperature 500 - 600 °C
 18.5 µm/m-°C
@Temperature 30.0 - 1100 °C
 19.0 µm/m-°C
@Temperature 600 - 700 °C
 19.5 µm/m-°C
@Temperature 700 - 800 °C
 20.0 µm/m-°C
@Temperature 800 - 900 °C
 21.0 µm/m-°C
@Temperature 900 - 1000 °C
 23.5 µm/m-°C
@Temperature 1000 - 1100 °C
Specific Heat Capacity 0.470 J/g-°C
@Temperature 20.0 °C
 0.485 J/g-°C
@Temperature 100 °C
 0.500 J/g-°C
@Temperature 200 °C
 0.520 J/g-°C
@Temperature 300 °C
 0.535 J/g-°C
@Temperature 400 °C
 0.555 J/g-°C
@Temperature 500 °C
 0.570 J/g-°C
@Temperature 600 °C
 0.585 J/g-°C
@Temperature 700 °C
 0.605 J/g-°C
@Temperature 800 °C
 0.620 J/g-°C
@Temperature 900 °C
 0.640 J/g-°C
@Temperature 1000 °C
 0.665 J/g-°C
@Temperature 1100 °C
Thermal Conductivity 12.0 W/m-K
@Temperature 20.0 °C
 13.0 W/m-K
@Temperature 100 °C
 15.0 W/m-K
@Temperature 200 °C
 16.0 W/m-K
@Temperature 300 °C
 18.0 W/m-K
@Temperature 400 °C
 20.0 W/m-K
@Temperature 500 °C
 22.0 W/m-K
@Temperature 600 °C
 23.0 W/m-K
@Temperature 700 °C
 25.0 W/m-K
@Temperature 800 °C
 27.0 W/m-K
@Temperature 900 °C
 28.0 W/m-K
@Temperature 1000 °C
 30.0 W/m-K
@Temperature 1100 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.10 %
Chromium, Cr 22.5 %
Cobalt, Co 1.5 %
Copper, Cu 3.0 %
Manganese, Mn 0.50 %
Nickel, Ni 25 %
Niobium, Nb (Columbium, Cb) 0.50 %
Nitrogen, N 0.23 %
Phosphorus, P <= 0.025 %
Silicon, Si 0.20 %
Sulfur, S <= 0.015 %
Tungsten, W 3.6 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ASTM A213 T9 9Cr-1Mo STEEL TUBES FOR BOILERS AND HEAT EXCHANGERS (STBA 26)

NSANDV5248 / 199812

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.