MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Envalior Stanyl® TW341-N PA46
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 46 (PA46)

Material Notes: Heat Stabilized, Lubricated

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.18 g/ccdry; ISO 1183
Moisture Absorption 3.70 %Sim. To ISO 62
Linear Mold Shrinkage, Flow 0.020 cm/cmSim. To ISO 294-4
Linear Mold Shrinkage, Transverse 0.020 cm/cmSm. To ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 55.0 MPacond; ISO 527-1/-2
 100 MPadry; ISO 527-1/-2
 30.0 MPa
@Temperature 200 °C
ISO 527-1/-2
 35.0 MPa
@Temperature 180 °C
ISO 527-1/-2
 40.0 MPa
@Temperature 160 °C
ISO 527-1/-2
 50.0 MPa
@Temperature 120 °C
ISO 527-1/-2
Elongation at Break 40 %dry; ISO 527-1/-2
 >= 50 %cond; ISO 527-1/-2
 >= 50 %
@Temperature 120 °C
ISO 527-1/-2
 >= 50 %
@Temperature 160 °C
ISO 527-1/-2
 >= 50 %
@Temperature 180 °C
ISO 527-1/-2
 >= 50 %
@Temperature 200 °C
ISO 527-1/-2
Tensile Modulus 1.00 GPacond; ISO 527-1/-2
 3.30 GPadry; ISO 527-1/-2
 0.500 GPa
@Temperature 200 °C
ISO 527-1/-2
 0.600 GPa
@Temperature 180 °C
ISO 527-1/-2
 0.650 GPa
@Temperature 160 °C
ISO 527-1/-2
 0.800 GPa
@Temperature 120 °C
ISO 527-1/-2
Flexural Modulus 900 MPacond; ISO 178
 3000 MPadry; ISO 178
 600 MPa
@Temperature 160 °C
ISO 178
 800 MPa
@Temperature 120 °C
ISO 178
Fatigue Strength 12.0 MPa
@# of Cycles 1.00e+8 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 21.0 MPa
@# of Cycles 1.00e+7 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 30.0 MPa
@# of Cycles 1.00e+6 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 35.0 MPa
@# of Cycles 100000 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 37.0 MPa
@# of Cycles 10000 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 39.0 MPa
@# of Cycles 1000 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
 41.0 MPa
@# of Cycles 100 ,
Temperature 140 °C
R = 0.1, 8 Hz, dry
Izod Impact Resistance 0.400 J/cm²
@Temperature -40.0 °C
cond; ISO 180/1A
 0.400 J/cm²
@Temperature -40.0 °C
dry; ISO 180/1A
 1.00 J/cm²
@Temperature 23.0 °C
dry; ISO 180/1A
 3.50 J/cm²
@Temperature 23.0 °C
cond; ISO 180/1A
Charpy Impact Unnotched NB
@Temperature 23.0 °C
cond; ISO 179/1eU
 NB
@Temperature -30.0 °C
cond; ISO 179/1eU
 NB
@Temperature 23.0 °C
dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
dry; ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²
@Temperature -30.0 °C
cond; ISO 179/1eA
 4.00 kJ/m²
@Temperature -30.0 °C
dry; ISO 179/1eA
 10.0 kJ/m²
@Temperature 23.0 °C
dry; ISO 179/1eA
 35.0 kJ/m²
@Temperature 23.0 °C
cond; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+9 ohm-cmcond; IEC 60093
 1.00e+15 ohm-cmdry; IEC 60093
Dielectric Strength 15.0 kV/mmcond; IEC 60243-1
 25.0 kV/mmdry; IEC 60243-1
Comparative Tracking Index 400 Vdry; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 85.0 µm/m-°Cdry; ISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°Cdry; ISO 11359-1/-2
Melting Point 295 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 152 °C5000 hours Thermal Index; IEC 60216/ISO 527-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 190 °Cdry; ISO 75-1/-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Envalior Stanyl® TW341-J PA46
BASF Ultramid® A3K BK 00464 PA66 (Conditioned)
Envalior Stanyl® TW341-B PA46
Envalior Stanyl® TW341 PA46, Dry, Heat Stabilized
Domo Technyl® A 218 V35 Nylon 66, 35% Glass Fiber, EH50

PDSM9888 / 161509

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.