MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Chemours Viton® GFLT-600S with CaO Fluoroelastomer Compound
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes:
  • Cures exceptionally fast to a high state of cure
  • Similar to improved low temperature properties compared to Viton® GFLT
  • Improved mold release/mold fouling properties
  • Improved mold flow and less shear sensitivity for a 65 Mooney peroxy cured FKM
  • Excellent physical properties with high elongation, both original and aged
  • Heat, fluids, and low temperature resistance comparable to Viton® GFLT
  • Improved water resistance/lower volume swell in water
  • Excellent compression set resistance with either low or no postcure

Chemours was formed from former DuPont performance chemicals businesses, including the Viton product line, in 2015.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6969No Postcure; ASTM D1414
 71712 hours Postcure; ASTM D1414
 71714 hours Postcure; ASTM D1414
Tensile Strength at Break 13.3 MPa1930 psiNo Postcure; ASTM D412
 16.6 MPa2410 psi4 hours Postcure; ASTM D412
 16.8 MPa2440 psi2 hours Postcure; ASTM D412
Tensile Stress at Strain  0.700 MPa
@Strain 10 %
102 psi
@Strain 10 %
No Postcure; ASTM D412
 0.700 MPa
@Strain 10 %
102 psi
@Strain 10 %
2 hours Postcure; ASTM D412
 0.800 MPa
@Strain 10 %
116 psi
@Strain 10 %
4 hours Postcure; ASTM D412
Elongation at Break 200 %200 %4 hours Postcure; ASTM D412
 213 %213 %2 hours Postcure; ASTM D412
 215 %215 %No Postcure; ASTM D412
100% Modulus  5.00 MPa
@Strain 100 %
725 psi
@Strain 100 %
No Postcure; ASTM D412
 5.90 MPa
@Strain 100 %
856 psi
@Strain 100 %
2 hours Postcure; ASTM D412
 6.00 MPa
@Strain 100 %
870 psi
@Strain 100 %
4 hours Postcure; ASTM D412
Compression Set  13 %
@Temperature 200 °C,
Time 79200 sec
13 %
@Temperature 392 °F,
Time 22.0 hour
O-Rings, no postcure; ASTM D395B
 14 %
@Temperature 200 °C,
Time 79200 sec
14 %
@Temperature 392 °F,
Time 22.0 hour
O-Rings, postcured 2hrs; ASTM D395B
 19 %
@Temperature 200 °C,
Time 252000 sec
19 %
@Temperature 392 °F,
Time 70.0 hour
O-Rings, postcured 2hrs; ASTM D395B
 20 %
@Temperature 200 °C,
Time 252000 sec
20 %
@Temperature 392 °F,
Time 70.0 hour
O-Rings no postcure; ASTM D395B
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg -25.3 °C-13.5 °F2 hours Postcure
 
Processing PropertiesMetricEnglishComments
Processing Temperature  177 °C
@Time 421 sec
351 °F
@Time 0.117 hour
Cure
 232 °C
@Time 7200 - 14400 sec
450 °F
@Time 2.00 - 4.00 hour
Postcure
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 67 %67 %Uncompounded Viton
 
Descriptive Properties
Compound NumberA44-05
Formulation as Tested100GFLT-600S
 2Varox® DBPH-50
 3CaO
 3Diak 7 (TAIC)
 30MT Black

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chemours Viton® GBLT-600S Fluoroelastomer Compound
Chemours Viton® GF-600S with 60-MT Black Fluoroelastomer Compound
Chemours Viton® GF-600S Fluoroelastomer Compound
Chemours Viton® GBLT-600S with 5-MT Black Fluoroelastomer Compound
Chemours Viton® GBL-600S with 5-MT Black Fluoroelastomer Compound

PDVC9850 / 170491

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.