MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

SABIC NORYL™ Resin HN731A Polyphenylene Ether + PS (PPE+PS)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ HN731A resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade is US FDA and European Food Contact approved, biocompatible (ISO10993 or USP Class VI), RoHS compliant, and It is subject to SABIC’s Healthcare management of change and formulation lock. NORYL HN731A resin exhibits good impact resistance, excellent hydrolytical stability, and chemical resistance. This light weight and colorable material is an excellent candidate for medical device and pharmaceutical applications such as drug-delivery inhalers.

Features: Hydrolytic Stability,Low Creep Sensitivity,Steam Sterilizable,Radiation Sterilizable,Gamma Sterilizable,Ethylene Oxide Sterilizable,E-beam Sterilizable,Low Warpage,Food Contact Acceptable,Biocompatible

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.06 g/cc1.06 g/ccASTM D792
Density 1.06 g/cc0.0383 lb/in³ISO 1183
Water Absorption 0.060 %
@Time 86400 sec
0.060 %
@Time 24.0 hour
ASTM D570
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.0600 %0.0600 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.23 %0.23 %ISO 62-1
Viscosity 8.0 cP
@Load 5.00 kg,
Temperature 280 °C
8.0 cP
@Load 11.0 lb,
Temperature 536 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 9.2 g/10 min
@Load 5.00 kg,
Temperature 280 °C
9.2 g/10 min
@Load 11.0 lb,
Temperature 536 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 119119ASTM D785
Tensile Strength at Break 49.0 MPa7110 psi50 mm/min; ASTM D638
 50.0 MPa7250 psi50 mm/min; ISO 527
Tensile Strength, Yield 55.0 MPa7980 psi50 mm/min; ISO 527
 58.0 MPa8410 psi50 mm/min; ASTM D638
Elongation at Break 28.1 %28.1 %50 mm/min; ASTM D638
 30 %30 %50 mm/min; ISO 527
Elongation at Yield 5.0 %5.0 %50 mm/min; ISO 527
 7.2 %7.2 %50 mm/min; ASTM D638
Tensile Modulus 2.30 GPa334 ksi1 mm/min; ISO 527
 2.86 GPa415 ksi50 mm/min; ASTM D638
Flexural Strength 75.0 MPa10900 psiyield, 2 mm/min; ISO 178
 89.0 MPa12900 psiyld, 2.6 mm/min, 100 mm span; ASTM D790
 90.0 MPa13100 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.20 GPa319 ksi2 mm/min; ISO 178
 2.42 GPa351 ksi2.6 mm/min, 100 mm span; ASTM D790
 2.64 GPa383 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 213 J157 ft-lbASTM D256
 133 J
@Temperature -40.0 °C
98.1 ft-lb
@Temperature -40.0 °F
ASTM D256
Izod Impact, Notched (ISO) 15.0 kJ/m²7.14 ft-lb/in²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 1.50 J/cm²7.14 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Gardner Impact  5.00 J
@Temperature -40.0 °C
3.69 ft-lb
@Temperature -40.0 °F
ASTM D3029
 25.0 J
@Temperature -30.0 °C
18.4 ft-lb
@Temperature -22.0 °F
ASTM D3029
Dart Drop, Total Energy 48.0 J35.4 ft-lbASTM D3763
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 2.65
@Frequency 50.0 - 60.0 Hz
2.65
@Frequency 50.0 - 60.0 Hz
ASTM D150
Dielectric Strength 21.6 kV/mm
@Thickness 3.20 mm
549 kV/in
@Thickness 0.126 in
in oil; ASTM D149
Dissipation Factor 0.00040
@Frequency 50.0 - 60.0 Hz
0.00040
@Frequency 50.0 - 60.0 Hz
ASTM D150
Arc Resistance 0.00 - 60 sec0.00 - 60 secASTM D495
Comparative Tracking Index 175 - 250 V175 - 250 VUL 746A
Hot Wire Ignition, HWI 30 - 60 sec30 - 60 secUL 746A
High Amp Arc Ignition, HAI >= 120 arcs>= 120 arcsUL 746A
High Voltage Arc-Tracking Rate, HVTR >= 150 mm/min>= 5.91 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 91.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
51.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow  70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 95.4 µm/m-°C
@Temperature -40.0 - 40.0 °C
53.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi)  131 °C
@Thickness 3.20 mm
268 °F
@Thickness 0.126 in
unannealed; ASTM D648
 137 °C
@Thickness 6.40 mm
279 °F
@Thickness 0.252 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 115 °C239 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 117 °C
@Thickness 3.20 mm
243 °F
@Thickness 0.126 in
unannealed; ASTM D648
 126 °C
@Thickness 6.40 mm
259 °F
@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point 135 °C275 °FRate B/50; ISO 306
 140 °C284 °FRate B/120; ISO 306
 148 °C298 °FRate B/50; ASTM D1525
UL RTI, Electrical 105 °C221 °FUL 746B
UL RTI, Mechanical with Impact 90.0 °C194 °FUL 746B
UL RTI, Mechanical without Impact 105 °C221 °FUL 746B
Flammability, UL94 HB
@Thickness 1.47 mm
HB
@Thickness 0.0579 in
UL 94
Oxygen Index 22 %22 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 280 - 310 °C536 - 590 °F
Zone 2 260 - 305 °C500 - 581 °F
Zone 3 270 - 310 °C518 - 590 °F
Melt Temperature 280 - 310 °C536 - 590 °FInjection Molding
Mold Temperature 75.0 - 105 °C167 - 221 °F
Drying Temperature 105 - 110 °C221 - 230 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 8.00 hour8.00 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 30 - 70 %30 - 70 %
Screw Speed 20 - 100 rpm20 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82334 / 290281

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.