MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
A. Schulman Diamond Centrex® 833 Sheet Extrusion Grade  (discontinued **)
Categories: Polymer; Thermoplastic; ASA Polymer

Material Notes: Centrex 833 resin is a high-gloss, high-impact grade of ASA (acrylonitrile-styrene-acrylate) with good resistance to weather aging. It has good melt strength for extrusion and thermoforming, and it can be easily coextruded. The recommended substrate is ABS (acrylonitrile-butadiene-styrene) resin.

Applications: Typical applications for Centrex 833 resin includes exterior parts requiring high gloss, such as spas; marine components, boat hulls and decks; doors, covers, and trim for recreational vehicles; swimming pool steps; and fiberglass-reinforced plastic replacements. As with any product, use of Centrex 833 resin in a given application must be tested (including but not limited to field testing) in advance by the user to determine suitability.

A. Schulman has acquired Network Polymers & Diamond Polymers.

Key Words: Weatherable Polymer
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.05 g/ccASTM D792
Melt Flow 8.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 89ASTM D785
Tensile Strength, Yield 31.7 MPachs 2.0 in/min; ASTM D638
Tensile Modulus 1600 MPachs 2.0 in/min; ASTM D638
Flexural Strength 51.7 MPachs 0.05 in/min; ASTM D790
Flexural Modulus 16000 MPatangent; chs 0.05 in/min; ASTM D790
Izod Impact, Notched 117 J/m
@Thickness 3.17 mm,
Temperature -30.0 °C
ASTM D256
 133 J/m
@Thickness 3.17 mm,
Temperature -18.0 °C
ASTM D256
 347 J/m
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D256
Impact Test 30.0 J
@Temperature -30.0 °C
ASTM D3763
 38.0 J
@Temperature -18.0 °C
ASTM D3763
 43.0 J
@Temperature 23.0 °C
ASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear 100 µm/m-°CASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 77.0 °C0.125";; ASTM D648
Flammability, UL94 HB
 
Optical PropertiesOriginal ValueComments
Gloss 75 - 85 %Formed; 60°; ASTM D523
 90 - 100 %Sheet; 60°; ASTM D523

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
A. Schulman Diamond Centrex® 485 Sheet Extrusion Grade
INEOS Styrolution Luran® S 797SE ASA
A. Schulman Diamond Centrex® 825 Sheet Extrusion Grade
A. Schulman Diamond Centrex® 835 Sheet Extrusion Grade

PDIAM357 / 126448

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.