SABIC LNP™ COLORCOMP™ Compound W1000Z Polybutylene Terephthalate (PBT)
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), Unreinforced, Molded
Material Notes:
LNP COLORCOMP W1000I compound is based on Polybutylene Terephthalate (PBT) resin. Added features of this grade include: High Viscosity suitable for Extrusion.
Features: Aesthetics and Appearance,Custom Color
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.31
g/cc
1.31
g/cc
ASTM D792
1.316
g/cc
1.316
g/cc
ASTM D792
Water Absorption
0.080 %
@Time 86400 sec
0.080 %
@Time 24.0 hour
ASTM D570
Moisture Absorption
0.0200 %
0.0200 %
Compounding Extrusion
Viscosity
9.0
cP
@Load 2.16 kg,
Temperature 250 °C
9.0
cP
@Load 4.76 lb,
Temperature 482 °F
MVR cc/10 min; ASTM D1238
9.0
cP
@Load 2.16 kg,
Temperature 250 °C
9.0
cP
@Load 4.76 lb,
Temperature 482 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow
0.0090
-
0.016
cm/cm
@Thickness 0.750 - 2.30 mm
0.0090
-
0.016
in/in
@Thickness 0.0295 - 0.0906 in
SABIC method
0.015
-
0.023
cm/cm
@Thickness 2.30 - 4.60 mm
0.015
-
0.023
in/in
@Thickness 0.0906 - 0.181 in
SABIC method
Linear Mold Shrinkage, Transverse
0.010
-
0.017
cm/cm
@Thickness 0.750 - 2.30 mm
0.010
-
0.017
in/in
@Thickness 0.0295 - 0.0906 in
SABIC method
0.016
-
0.024
cm/cm
@Thickness 2.30 - 4.60 mm
0.016
-
0.024
in/in
@Thickness 0.0906 - 0.181 in
SABIC method
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
117
117
ASTM D785
Tensile Strength, Yield
51.0
MPa
7400
psi
50 mm/min; ASTM D638
Elongation at Break
300 %
300 %
50 mm/min; ASTM D638
Flexural Strength
82.0
MPa
11900
psi
yld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus
2.34
GPa
339
ksi
1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched
53.0
J
39.1
ft-lb
ASTM D256
Izod Impact, Unnotched
16.02
J/cm
30.01
ft-lb/in
ASTM D4812
Gardner Impact
40.0
J
29.5
ft-lb
ASTM D3029
Electrical Properties
Metric
English
Comments
Volume Resistivity
>=
4.00e+16
ohm-cm
>=
4.00e+16
ohm-cm
ASTM D257
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
81.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
45.0
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
140
µm/m-°C
@Temperature 60.0 - 138 °C
77.8
µin/in-°F
@Temperature 140 - 280 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi)
154
°C
@Thickness 6.40 mm
309
°F
@Thickness 0.252 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
54.0
°C
@Thickness 6.40 mm
129
°F
@Thickness 0.252 in
unannealed; ASTM D648
Processing Properties
Metric
English
Comments
Processing Temperature
25.0
-
35.0
°C
77.0
-
95.0
°F
Water Bath Temperature
Zone 1
200
-
230
°C
392
-
446
°F
Compounding Extrusion
Zone 2
240
-
255
°C
464
-
491
°F
Compounding Extrusion
Zone 3
240
-
275
°C
464
-
527
°F
Compounding Extrusion
Zone 4
240
-
275
°C
464
-
527
°F
Compounding Extrusion
Adapter Temperature
240
-
275
°C
464
-
527
°F
Compounding Extrusion
Die Temperature
240
-
275
°C
464
-
527
°F
Compounding Extrusion
Melt Temperature
245
-
260
°C
473
-
500
°F
Compounding Extrusion
Drying Temperature
110
-
120
°C
230
-
248
°F
Compounding Extrusion
Dry Time
4.00
-
6.00
hour
4.00
-
6.00
hour
Compounding Extrusion
8.00
hour
8.00
hour
Cumulative; Compounding Extrusion
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH80581 / 288528
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.