MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Toray TOYOLAC™ ABS Resin AX05-X03 ABS Polymer, Detergent Resistant
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Detergent resistant, standard, ABS.

General Toyolac™ Notes: TOYOLAC™ ABS is a versatile thermoplastic consisting of acrylonitrile, butadiene, and styrene and it has unique set of properties combining strength, lightness, and aesthetics. TOYOLAC™ is widely used in both industrial and household goods due to its excellent mechanical, chemical, electrical properties, and superior processability.

Information provided by Toray Resin Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/in23°C/50% RH; Toray Method
Melt Flow 15 g/10 min
@Load 9.99 kg,
Temperature 220 °C
15 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R  108
@Temperature 23.0 °C
108
@Temperature 73.4 °F
50% RH; ASTM D785
 108
@Temperature 23.0 °C
108
@Temperature 73.4 °F
ISO 2039-2
Tensile Strength 43.0 MPa6240 psiASTM D638
 41.0 MPa
@Temperature 23.0 °C
5950 psi
@Temperature 73.4 °F
ISO 527-1,2
Elongation at Break 25 %25 %ASTM D638
 15 %
@Temperature 23.0 °C
15 %
@Temperature 73.4 °F
ISO 527-1,2
Flexural Strength 64.0 MPa9280 psiASTM D790
 60.0 MPa
@Temperature 23.0 °C
8700 psi
@Temperature 73.4 °F
ISO 178
Flexural Modulus 2.00 GPa290 ksiASTM D790
 1.86 GPa
@Temperature 23.0 °C
270 ksi
@Temperature 73.4 °F
50% RH; ISO 178
Izod Impact, Notched  3.40 J/cm
@Thickness 12.7 mm,
Temperature 23.0 °C
6.37 ft-lb/in
@Thickness 0.500 in,
Temperature 73.4 °F
V-notched; ASTM D256
 4.80 J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
8.99 ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
V-notched; ASTM D256
Charpy Impact, Notched 3.40 J/cm²
@Temperature 23.0 °C
16.2 ft-lb/in²
@Temperature 73.4 °F
V-Notched; ISO 179
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 79.0 °C174 °FISO 75-1,2
 84.0 °C183 °FUnannealed; ASTM D648
Vicat Softening Point 90.0 - 95.0 °C194 - 203 °F
Flammability, UL94 HBHB

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTORAY9208 / 248897

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.