MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ASTM A213 T11 Alloy Steel, Chromium Molybdenum, F11-1
Categories: Metal; Ferrous Metal; ASTM Steel; Tool Steel; Cold Work Steel

Material Notes: 1.25Cr-0.5Mo-Si STEEL TUBES FOR BOILERS AND HEAT EXCHANGERS (STBA 23)

Creep and rupture data provided by NIMS

Key Words: JIS G3462 STBA 23; UNS K22597; BS 3606 621
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.85 g/ccBased on UNS number
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 415 MPa
Tensile Strength, Yield 205 MPa
Elongation at Break 30 %
Rupture Strength 28.0 - 47.0 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
 58.0 - 68.0 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
 84.0 - 92.0 MPa
@Temperature 525 °C,
Time 3.60e+8 sec
 117 - 135 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.050 - 0.15 %
Chromium, Cr 1.0 - 1.5 %
Iron, Fe 96.05 - 97.71 %
Manganese, Mn 0.30 - 0.60 %
Molybdenum, Mo 0.44 - 0.65 %
Phosphorus, P <= 0.025 %
Silicon, Si 0.50 - 1.0 %
Sulfur, S <= 0.025 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ASTM A213 T22 2.25Cr-1Mo STEEL FOR BOILER AND HEAT EXCHANGER SEAMLESS TUBES (STBA 24)
ASTM A213 T12 Alloy Steel, Chromium Molybdenum
ASTM A213 T9 9Cr-1Mo STEEL TUBES FOR BOILERS AND HEAT EXCHANGERS (STBA 26)
AISI 4012 Steel
ASTM A213 T5 5Cr-0.5Mo STEEL TUBES FOR BOILERS AND HEAT EXCHANGERS (STBA 25)

NIMS011 / 77528

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.