Addiplast Addinyl C2 V15 Nylon 66/6, 15% Glass Filled
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6/66
;
Nylon 66/6, 20% Glass Fiber Reinforced
Material Notes:
Glass fiber reinforced, high strength
Information provided by Addiplast.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.25
g/cc
0.0452
lb/in³
ISO 1183/A
Mechanical Properties
Metric
English
Comments
Hardness, Shore D
77
77
Conditioned; ISO 868
84
84
ISO 868
Tensile Strength at Break
80.0
MPa
11600
psi
Conditioned; ISO R 527
130
MPa
18900
psi
ISO R 527
Elongation at Yield
4.0 %
4.0 %
ISO R 527
10 %
10 %
Conditioned; ISO R 527
Modulus of Elasticity
3.00
GPa
435
ksi
Conditioned; ISO 178
5.50
GPa
798
ksi
ISO 178
Izod Impact, Notched (ISO)
6.00
kJ/m²
2.86
ft-lb/in²
ISO 180/1A
11.0
kJ/m²
5.23
ft-lb/in²
Conditioned; ISO 180/1A
Charpy Impact Unnotched
3.50
J/cm²
16.7
ft-lb/in²
ISO 179/IeU
5.50
J/cm²
26.2
ft-lb/in²
Conditioned; ISO 179/IeU
Charpy Impact, Notched
0.550
J/cm²
2.62
ft-lb/in²
ISO 179/IeA
0.800
J/cm²
3.81
ft-lb/in²
Conditioned; ISO 179/IeA
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+12
ohm-cm
1.00e+12
ohm-cm
Conditioned; CEI 60093
1.00e+15
ohm-cm
1.00e+15
ohm-cm
CEI 60093
Dielectric Strength
30.0
kV/mm
762
kV/in
Conditioned; CEI 60243-1
32.0
kV/mm
813
kV/in
CEI 60243-1
Comparative Tracking Index
600
V
600
V
CEI 60112/Solution A
Thermal Properties
Metric
English
Comments
CTE, linear
35.0
µm/m-°C
19.4
µin/in-°F
ASTM E831
Melting Point
243
°C
469
°F
ISO 3146/C2
Deflection Temperature at 1.8 MPa (264 psi)
230
°C
446
°F
ISO 75-2/AF
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Celanese Zytel® HTN52G45HSL BK083 PA6T/66-GF45
Celanese Zytel® 74G33J NC010 PA66+PA6-GF33
Celanese Nilit FRIANYL C73 HS28 Nylon 6.6/6 for injection molding
BASF Ultramid® C33 PA6/66
BASF Ultramid® C33 01 PA66/6 (Dry)
PFADD885 / 156099
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.