MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
DuPont Elvax® 40L-03 Strippable Semiconductive Insulation Shield Formulation  (discontinued **)
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate

Material Notes: Elvax® 40L-03 strippable semiconductive insulation shield.

Information provided by DuPont.

This product line/trade name was acquired by Dow, but this specific grade was discontinued prior to the acquisition.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 10.89 MPaAfter 7 days/121°C air oven, ASTM D573
 12.1 MPaASTM D412
Elongation at Break 210 %After 7 days/121°C air oven; ASTM D573
 250 %ASTM D412
Tear Strength 8.50 kN/mASTM D470
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 116 ohm-cm
@Temperature 130 °C
ASTM D991-82
 174 ohm-cm
@Temperature 23.0 °C
ASTM D991-82
 179 ohm-cm
@Temperature 90.0 °C
ASTM D991-82
 
Descriptive Properties
Antioxidant1.5 phr
Conductive Black50 phr
Dicumyl Peroxide2.5 phr
Elvax® 40L-03100 phr
Stearic Acid1 phr
Triallyl Cyanurate1 phr

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Elvax® 3169 Ethylene-Vinyl Acetate Copolymer Resin for Coextrusion, Blown Film
DuPont Elvax® 3136 Ethylene-Vinyl Acetate Copolymer Resin for Blown Film
DuPont Elvax® 3134Q Ethylene-Vinyl Acetate Copolymer Resin for Extrusion Coating, Casting
DuPont Elvax® 3130SBZ Ethylene-Vinyl Acetate Copolymer Resin for Blown Film
DuPont Elvax® 3130SB Ethylene-Vinyl Acetate Copolymer Resin for Blown Film

PDUPM115 / 33782

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.