MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Materia Proxima® ACR 4100 Polydicyclopentadiene Thermoset Resin
Categories: Polymer; Thermoset; Polydicyclopentadiene (PDCPD)

Material Notes: Proxima ACR 4100 is an ultra-low viscosity resin designed for infusion processes with commercial fabrics based on glass roving and carbon fiber tow. It provides laminates exhibiting excellent fracture toughness, low water absorption and a glass transition temperature above 120 °C.

Proxima® HPR High Performance Resins are designed to deliver the right combination of thermal and mechanical properties, in an easy to process system. Proxima® HPR resins offer better thermal stability than standard thermoplastics and better wear resistance than typical compression-molded thermosets, while delivering corrosion resistance, good machinability, a wide use-temperature range, and ease of fabrication.

Proxima® HPR resins are two-part liquid thermosetting systems created with proprietary blends of dicyclopentadiene (DCPD) and other norbornene monomers which are thermally activated by Grubbs Catalyst® technology. Proxima® HPR resins are specially designed to have a low viscosity for fast and easy mold fill. As a result, Proxima® resins can be processed by most standard thermoset processing techniques such as mold-casting, spin-casting, reaction-injection molding, and coating.

Information provided by Materia, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccPolymer; ASTM D792
Water Absorption <= 1.0 %
@Temperature 100 °C
ASTM D570
Brookfield Viscosity 7.0 cP
@Temperature 30.0 °C
Resin
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 69.0 MPaASTM D638
Elongation at Break 11 %ASTM D638
Tensile Modulus 2.55 GPaASTM D638
Flexural Strength 105 MPaASTM D790
Flexural Modulus 2540 MPaASTM D790
Compressive Strength 96.0 MPaASTM D695
Compressive Modulus 2160 MPaASTM D695
Fracture Toughness 2.60 MPa-m½KIC; ASTM D5045
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg 120 °CDSC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Materia Proxima® HPR 2000 Polydicyclopentadiene Thermoset Resin
Overview of materials for Polydicyclopentadiene (PDCPD)
Materia Proxima® HPR 2012 Polydicyclopentadiene Thermoset Resin
Materia Proxima® HPR 2013 Polydicyclopentadiene Thermoset Resin
Lubrizol Telene 1610 A/B & A/BK Dicyclopentadiene (DCPD)

PMATERI970 / 192540

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.