MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Röchling SUSTARIN® C ESD 90 POM/Acetal Copolymer-Static Dissipative
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Unreinforced

Material Notes:
  • Antistatic
  • No Carbon black
  • Good sliding behavior
Product applications:
  • Clean room and semi conductor industry
  • Explosion protection
  • Packaging industry

Information provided by Röchling.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.33 g/cc0.0480 lb/in³ASTM D792
Water Absorption 1.0 %
@Time 86400 sec
1.0 %
@Time 24.0 hour
ASTM D570
Water Absorption at Saturation 2.0 %2.0 %ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8686ASTM D785
Hardness, Rockwell R 120120ASTM D785
Hardness, Shore D 8686ASTM D2240
Tensile Strength, Yield 75.8 MPa11000 psiASTM D638
Elongation at Break 30 %30 %ASTM D638
Tensile Modulus 2.93 GPa425 ksiASTM D638
Flexural Strength 124 MPa18000 psiASTM D790
Flexural Modulus 3.10 GPa450 ksiASTM D790
Compressive Strength 55.2 MPa8000 psiASTM D695
Izod Impact, Notched 0.534 - 0.961 J/cm1.00 - 1.80 ft-lb/inASTM D256
Coefficient of Friction, Dynamic 0.200.20
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square 1.00e+9 - 1.00e+10 ohm1.00e+9 - 1.00e+10 ohmASTM D257
Dielectric Constant 3.7
@Frequency 1e+6 Hz
3.7
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 15.7 kV/mm399 kV/inASTM D149
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
0.0050
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 86.4 µm/m-°C48.0 µin/in-°FASTM D696
Thermal Conductivity 0.245 W/m-K1.70 BTU-in/hr-ft²-°F
Melting Point 166 °C330 °F
Maximum Service Temperature, Air 82.2 °C180 °F
Deflection Temperature at 1.8 MPa (264 psi) 121 °C250 °FASTM D648
Flammability, UL94 HB
@Thickness 3.17 mm
HB
@Thickness 0.125 in
 
Compliance PropertiesMetricEnglishComments
FDA NoNo
NSF NoNo
USDA NoNo

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Röchling SUSTARIN® C POM/Acetal Copolymer

PROCH9029 / 232732

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.