MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Total PPH 3925WZ Polypropylene, Injection Molding Grade
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Easy flow injection molding homopolymer

Nucleation - FINA 3925WZ is nucleated to provide fast cycle time and improve contact clarity.

Antistat - FINA 3925WZ contains an antistat that will help protect molded parts from shelf dusting.

FDA - FINA 3925WZ complies with all applicable FDA regulations for food contact applications.

Recommended Applications - FINA 3925WZ is recommended for thin wall parts, caps and closures in multi-cavity molds.

Processing - FINA 3925WZ resin processes on conventional injection molding equipment with typical melt temperatures of 390- 450°F (200-232°C)

Data provided by the manufacturer, Total Petrochemicals.

Total Petrochemicals acquired former Fina and Atofina plastics product lines.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.905 g/ccASTM D1505
Melt Flow 60 g/10 minASTM D1238L
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 107ASTM D288A
Tensile Strength, Ultimate 37.9 MPaASTM D638
Elongation at Break 6.0 %ASTM D638
Modulus of Elasticity 1.79 GPaASTM D638
Flexural Modulus 1.655 GPaASTM D790
Izod Impact, Notched 0.214 J/cmASTM D256A
Izod Impact, Unnotched 8.55 J/cmASTM D256A
 
Thermal PropertiesOriginal ValueComments
Melting Point 165 °CDSC
Deflection Temperature at 0.46 MPa (66 psi) 127 °CASTM D648
 
Processing PropertiesOriginal ValueComments
Melt Temperature 200 - 232 °CInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Braskem H 107 Injection Molding Polypropylene
LyondellBasell Pro-fax™ PH835 Polypropylene Homopolymer
Formosa Plastics Formolene® 6501A Blow Molding and Injection Molding Polypropylene
Formosa Plastics Formolene® 6502A Blow Molding and Injection Molding Polypropylene
Total PPH 3825WZ Polypropylene, Injection Molding Grade

PFIN76 / 38406

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.