MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Solvay CYCOM® 950 Epoxy Prepreg with Hy-E HS/950
Categories: Polymer; Thermoset; Epoxy

Material Notes: CYCOM® 950 resin is a 250 – 300°F (121 – 149°C) curing epoxy resin with good 220°F (104°C) dry service capability. It can be impregnated via hot melt or solution techniques on all available fibers and fabrics. CYCOM 950 is formulated for shrink tape processing, but it has been successfully processed by autoclave, press molding and vacuum bagging. Unidirectional tape and woven fabric impregnated with CYCOM 950 resin will retain excellent tack and drape for at least 10 days at 72°F (22°C). Standard cure is for 90 minutes at 275°F (135°C). No post cure is required for 220°F (104°C) dry service capability. The recommended autoclave lay-up procedure for this material is L-3 or L-6. The recommended cure procedure is C-6 or C-7 at 275°F (135°C).

Features & Benefits:

  • Available in a broad range of fibers and forms including tape, fabric and roving
  • Self-adhesive
  • Low flow
  • 220°F (104°C) dry and 180°F (82°C) wet service temperature
  • Laminate and sandwich panel usage
  • Multiprocessing capable: shrink tape, autoclave, press mold, vacuum bag
  • Shelf life of 6 months at 0°F (-18°C), 10 days at 72°F (22°C)
Applications: Tubular structures such as fishing rods, golf shafts and bike components

Typical Properties of CYCOM 950 Composite Laminate with High Modulus (48 – 58 Msi/331 – 400 GPa Class) Unidirectional Tape and Roving - CEM Product Code Hy-E HS/950

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 2550 - 2760 MPa370000 - 400000 psi
Elongation at Break 1.2 - 1.4 %1.2 - 1.4 %
Tensile Modulus 179 - 207 GPa26000 - 30000 ksi
Flexural Strength 62.1 - 75.8 MPa9000 - 11000 psi90°
 1480 - 1590 MPa215000 - 230000 psi
Flexural Modulus 6.89 - 8.27 GPa999 - 1200 ksi90°
 166 - 186 GPa24100 - 27000 ksi
Compressive Strength 1206 - 1413 MPa174900 - 204900 psi
Compressive Modulus 179 - 200 GPa26000 - 29000 ksi
Shear Strength 82.7 - 96.5 MPa12000 - 14000 psiShort Beam
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 82.0 °C180 °Fwet
 104 °C219 °Fdry
 
Processing PropertiesMetricEnglishComments
Processing Temperature 121 - 149 °C250 - 300 °FStandard cure is 90 min. at 275°F.
Shelf Life  0.333 Month
@Temperature 22.2 °C
0.333 Month
@Temperature 72.0 °F
Epoxy
 6.00 Month
@Temperature -17.8 °C
6.00 Month
@Temperature 0.000 °F
Epoxy

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay APC-2/AS4 PEEK Plus Carbon Fiber Reinforced Unidirectional Tape

PCYTED098d / 233306

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.