MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Acrylic, Optical Grade, Molded
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, Optical Grade, Molded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Acrylic, Optical Grade, Molded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.11 - 1.19 g/cc0.0401 - 0.0430 lb/in³Average value: 1.18 g/cc Grade Count:131
Water Absorption 0.300 %0.300 %Average value: 0.300 % Grade Count:24
Water Absorption at Saturation 0.300 - 2.00 %0.300 - 2.00 %Average value: 0.867 % Grade Count:3
Particle Size 230 - 600 µm230 - 600 µmAverage value: 538 µm Grade Count:6
Viscosity  2.00e+6 - 2.00e+6 cP
@Temperature 240 - 240 °C
2.00e+6 - 2.00e+6 cP
@Temperature 464 - 464 °F
Average value: 2.00e+6 cP Grade Count:1
 2.00e+6 - 2.00e+6 cP
@Shear Rate 100 - 100 1/s
2.00e+6 - 2.00e+6 cP
@Shear Rate 100 - 100 1/s
Average value: 2.00e+6 cP Grade Count:1
Linear Mold Shrinkage 0.00200 - 0.00800 cm/cm0.00200 - 0.00800 in/inAverage value: 0.00420 cm/cm Grade Count:128
Melt Flow 0.700 - 40.0 g/10 min0.700 - 40.0 g/10 minAverage value: 10.5 g/10 min Grade Count:131
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 48.0 - 99.048.0 - 99.0Average value: 85.6 Grade Count:31
Tensile Strength, Ultimate 38.0 - 89.3 MPa5510 - 13000 psiAverage value: 59.7 MPa Grade Count:124
Tensile Strength, Yield 54.0 - 72.0 MPa7830 - 10400 psiAverage value: 67.5 MPa Grade Count:8
Elongation at Break 2.00 - 40.0 %2.00 - 40.0 %Average value: 8.79 % Grade Count:125
Elongation at Yield 2.00 - 6.00 %2.00 - 6.00 %Average value: 3.65 % Grade Count:10
Modulus of Elasticity 1.76 - 3.65 GPa255 - 530 ksiAverage value: 2.87 GPa Grade Count:122
Flexural Yield Strength 48.3 - 124 MPa7000 - 18000 psiAverage value: 95.0 MPa Grade Count:131
Flexural Modulus 2.00 - 82.0 GPa290 - 11900 ksiAverage value: 6.73 GPa Grade Count:21
Izod Impact, Notched 0.160 - 1.30 J/cm0.300 - 2.44 ft-lb/inAverage value: 0.302 J/cm Grade Count:124
 0.26695 - 0.800 J/cm
@Temperature 0.000 - 0.000 °C
0.50011 - 1.50 ft-lb/in
@Temperature 32.0 - 32.0 °F
Average value: 0.516 J/cm Grade Count:3
 0.26695 - 0.800 J/cm
@Diameter 6.35 - 6.35 mm
0.50011 - 1.50 ft-lb/in
@Diameter 0.250 - 0.250 in
Average value: 0.516 J/cm Grade Count:3
Izod Impact, Notched (ISO) 1.70 - 2.20 kJ/m²0.809 - 1.05 ft-lb/in²Average value: 1.85 kJ/m² Grade Count:6
Charpy Impact Unnotched 1.80 - 2.60 J/cm²8.57 - 12.4 ft-lb/in²Average value: 2.00 J/cm² Grade Count:6
Charpy Impact, Notched 0.200 - 1.80 J/cm²0.952 - 8.57 ft-lb/in²Average value: 0.592 J/cm² Grade Count:9
Gardner Impact 0.226 - 9.04 J0.167 - 6.67 ft-lbAverage value: 1.55 J Grade Count:104
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 3.40 - 3.803.40 - 3.80Average value: 3.67 Grade Count:8
Dielectric Strength 18.0 - 45.0 kV/mm457 - 1140 kV/inAverage value: 21.4 kV/mm Grade Count:8
Dissipation Factor 0.0400 - 0.05000.0400 - 0.0500Average value: 0.0471 Grade Count:7
 
Thermal PropertiesMetricEnglishComments
CTE, linear 30.0 - 120 µm/m-°C16.7 - 66.7 µin/in-°FAverage value: 68.4 µm/m-°C Grade Count:125
 72.0 - 72.0 µm/m-°C
@Temperature 0.000 - 156 °C
40.0 - 40.0 µin/in-°F
@Temperature 32.0 - 312 °F
Average value: 72.0 µm/m-°C Grade Count:2
Specific Heat Capacity 1.30 - 1.50 J/g-°C0.311 - 0.359 BTU/lb-°FAverage value: 1.44 J/g-°C Grade Count:11
 1.90 - 2.30 J/g-°C
@Temperature 100 - 175 °C
0.454 - 0.550 BTU/lb-°F
@Temperature 212 - 347 °F
Average value: 2.10 J/g-°C Grade Count:3
Thermal Conductivity 0.190 - 0.220 W/m-K1.32 - 1.53 BTU-in/hr-ft²-°FAverage value: 0.205 W/m-K Grade Count:11
Melting Point 132 - 157 °C270 - 315 °FAverage value: 150 °C Grade Count:7
Maximum Service Temperature, Air 50.0 - 100 °C122 - 212 °FAverage value: 78.1 °C Grade Count:61
Deflection Temperature at 0.46 MPa (66 psi) 91.0 - 106 °C196 - 223 °FAverage value: 100 °C Grade Count:7
Deflection Temperature at 1.8 MPa (264 psi) 60.0 - 104 °C140 - 220 °FAverage value: 85.4 °C Grade Count:131
Vicat Softening Point 75.6 - 117 °C168 - 243 °FAverage value: 102 °C Grade Count:122
Flammability, UL94 HBHBGrade Count:80
Glow Wire Test 650 °C1200 °FAverage value: 650 °C Grade Count:6
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.49 - 1.511.49 - 1.51Average value: 1.49 Grade Count:22
Haze 0.400 - 12.0 %0.400 - 12.0 %Average value: 1.40 % Grade Count:120
Yellow Index -0.400 - 1.00 %-0.400 - 1.00 %Average value: 0.750 % Grade Count:8
Transmission, Visible 84.0 - 92.0 %84.0 - 92.0 %Average value: 91.6 % Grade Count:130
UV Transmittance 49.5 - 92.0 %49.5 - 92.0 %Average value: 77.6 % Grade Count:5
 
Processing PropertiesMetricEnglishComments
Melt Temperature 193 - 260 °C380 - 500 °FAverage value: 233 °C Grade Count:8
Mold Temperature 26.7 - 79.4 °C80.0 - 175 °FAverage value: 55.0 °C Grade Count:7
Drying Temperature 71.1 - 79.4 °C160 - 175 °FAverage value: 77.5 °C Grade Count:7

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acrylic, General Purpose, Molded
Overview of materials for Acrylic, Optical Sheet
Overview of materials for Acrylic, Cast
Overview of materials for Acrylic, Extruded
Overview of materials for Acrylic, Heat Resistant, Molded

O1306 / 77865

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.