MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AGC Fluon® P-66P PFA Resin
Categories: Polymer; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA)

Material Notes: Fluon® PFA (perfluoroalkoxy) is a melt-processible copolymer of tetrafluoroethylene and a perfluorinated vinyl ether. Fluon® PFA has chemical, electrical, and thermal properties almost identical to its close chemical cousin, polytetrafluoroethylene (PTFE), yet can be processed by conventional extrusion, injection molding, blow molding, and transfer molding techniques. This unique material can be used over a wide range of temperatures (-200°C to 260°C). It is available as a 1/8” pellet.

Benefits:

  • High Resistance to Heat
  • Excellent Chemical Resistance
  • Low Smoke and Flame Characteristics. Fluon® PFA is rated 94V-0 by Underwriters Laboratories Inc.
  • Outstanding Resistance to Weather and Aging
  • Excellent Dielectric Properties
  • Non-Stick Characteristics
Applications:
  • Tubing and Pipe
  • Film and Sheets
  • Valves, Fittings, and Housings
  • Wire and Cable

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.14 g/cc2.14 g/ccASTM D792
Water Absorption <= 0.030 %
@Time 86400 sec
<= 0.030 %
@Time 24.0 hour
ASTM D570
Melt Flow 2.0 g/10 min2.0 g/10 minASTM D3159
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6060ASTM D2240
Tensile Strength  13.8 MPa
@Temperature 250 °C
2000 psi
@Temperature 482 °F
ASTM D638
 39.0 MPa
@Temperature 23.0 °C
5660 psi
@Temperature 73.4 °F
ASTM D638
 50.0 MPa
@Temperature -79.0 °C
7250 psi
@Temperature -110 °F
 100 MPa
@Temperature -129 °C
14500 psi
@Temperature -200 °F
 130 MPa
@Temperature -198 °C
18900 psi
@Temperature -324 °F
Elongation at Break  1.0 %
@Temperature -198 °C
1.0 %
@Temperature -324 °F
 1.0 %
@Temperature -129 °C
1.0 %
@Temperature -200 °F
 9.0 %
@Temperature -79.0 °C
9.0 %
@Temperature -110 °F
 340 %
@Temperature 23.0 °C
340 %
@Temperature 73.4 °F
ASTM D638
 740 %
@Temperature 250 °C
740 %
@Temperature 482 °F
ASTM D638
Flexural Strength  3.00 MPa
@Temperature 250 °C
435 psi
@Temperature 482 °F
ASTM D790
 7.50 MPa
@Temperature 100 °C
1090 psi
@Temperature 212 °F
ASTM D790
 17.0 MPa
@Temperature 25.0 °C
2470 psi
@Temperature 77.0 °F
ASTM D790
Flexural Modulus  0.150 GPa
@Temperature 100 °C
21.8 ksi
@Temperature 212 °F
ASTM D790
 0.600 GPa
@Temperature 25.0 °C
87.0 ksi
@Temperature 77.0 °F
ASTM D790
 1.50 GPa
@Temperature -79.0 °C
218 ksi
@Temperature -110 °F
 3.90 GPa
@Temperature -129 °C
566 ksi
@Temperature -200 °F
Flex Crack Resistance 500000500000Cycles per MIT Folding Endurance; ASTM D2176
Izod Impact, Notched  7.00 J/cm
@Temperature -40.0 °C
13.1 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ASTM C256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+18 ohm-cm>= 1.00e+18 ohm-cmASTM D257
Dielectric Constant 2.07
@Frequency 1e+6 Hz
2.07
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 74.8 kV/mm1900 kV/inASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear  >= 90.0 µm/m-°C
@Temperature -100 - -75.0 °C
>= 50.0 µin/in-°F
@Temperature -148 - -103 °F
ASTM D696
 >= 120 µm/m-°C
@Temperature -75.0 - -15.0 °C
>= 66.7 µin/in-°F
@Temperature -103 - 5.00 °F
ASTM D696
 130 µm/m-°C
@Temperature 0.000 - 100 °C
72.0 µin/in-°F
@Temperature 32.0 - 212 °F
ASTM D696
 >= 140 µm/m-°C
@Temperature -15.0 - 100 °C
>= 77.8 µin/in-°F
@Temperature 5.00 - 212 °F
ASTM D696
 >= 160 µm/m-°C
@Temperature 100 - 150 °C
>= 88.9 µin/in-°F
@Temperature 212 - 302 °F
ASTM D696
 >= 210 µm/m-°C
@Temperature 150 - 210 °C
>= 117 µin/in-°F
@Temperature 302 - 410 °F
ASTM D696
Specific Heat Capacity 1.05 J/g-°C0.251 BTU/lb-°F
Melting Point 310 °C590 °FASTM D3459
Maximum Service Temperature, Air 260 °C500 °F
Deflection Temperature at 0.46 MPa (66 psi) 91.0 °C196 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 56.0 °C133 °FASTM D648
Vicat Softening Point 287 °C549 °F50°C/h; JIS K7206
Flammability, UL94 V-0V-0
Oxygen Index >= 95 %>= 95 %ASTM D2863
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.351.35ASTM D542
 
Descriptive Properties
Heat of Combustion2200 BTU/lbASTM D240

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AGC Fluon® P-65P PFA Resins
AGC Fluon® P-63P PFA Resin
AGC Fluon® P-62XP PFA Resin
Honeywell ACLAR® CX 130E Heat Sealable PCTFE Film
AGC Fluon® P-802UP PFA Perfluoropolymer

PAGCX257 / 191366

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.