MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Latrobe Lescalloy® D6AC VAC-ARC High Strength Alloy Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: LESCALLOY D6AC VAC-ARC steel is a medium carbon, low alloy, ultra high strength steel primarily designed for high strength structural applications requiring strength leaves up to 280,000 psi. This alloy provides a high yield strength to tensile strength ratio, combined with good ductility. A tough and fibrous fracture is exhibited to as low as -210°F in impact testing; also the notch toughness is excellent. It has been selected for fracture toughness critical applications at a variety of strength levels. The deep hardening characteristics of D6AC steel make it applicable for fairly large sections. Lescalloy D6AC VAC-ARC steel is produced by the consumable electrode vacuum arc remelting process to provide optimum cleanliness and preferred ingot structure, which in turn provide optimum transverse mechanical properties.

Heat Treatment - Austenitized at 1650°F. Oil quenched and air cooled, or salt quenched at 400-425°F for 10 minutes and air cooled

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.86 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 3636650°C Temper
 4646510°C Temper Temperature
 5353316°C Temper Temperature
Tensile Strength, Ultimate 1570 MPa228000 psi510°C Temper Temperature
 1930 MPa280000 psi316°C Temper Temperature
Tensile Strength, Yield 1345 MPa195100 psi510°C Temper Temperature
 1724 MPa250000 psi316°C Temper Temperature
Elongation at Break 7.0 %7.0 %316°C Temper Temperature
 7.0 %7.0 %510°C Temper Temperature
Reduction of Area 23 %23 %316°C Temper Temperature
 25 %25 %510°C Temper Temperature
Modulus of Elasticity 210 GPa30500 ksi
 76.5 GPa
@Temperature 649 °C
11100 ksi
@Temperature 1200 °F
 163 GPa
@Temperature 427 °C
23700 ksi
@Temperature 801 °F
Machinability 50 - 55 %50 - 55 %AISI B1112 Screw Stock
 
Thermal PropertiesMetricEnglishComments
CTE, linear  13.16 µm/m-°C
@Temperature 38.0 - 93.0 °C
7.311 µin/in-°F
@Temperature 100 - 199 °F
 16.1 µm/m-°C
@Temperature 316 - 704 °C
8.95 µin/in-°F
@Temperature 601 - 1300 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.46 %0.46 %
Chromium, Cr 1.1 %1.1 %
Iron, Fe 95.74 %95.74 %
Manganese, Mn 0.75 %0.75 %
Molybdenum, Mo 1.0 %1.0 %
Nickel, Ni 0.60 %0.60 %
Silicon, Si 0.25 %0.25 %
Vanadium, V 0.10 %0.10 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® Vasco® D6AC Specialty Steel, Heat Treatment: 913°C (1675°F) Q+T
ATI Allvac® Nickelvac® D6AC UNS K24728 Specialty Steel
Latrobe Lescalloy® 300M - HS VAC-ARC High Strength Alloy Steel
Latrobe Lescalloy® 4340 VAC-ARC ; 3.5" round High Strength Alloy Steel
AISI 4340 Steel, annealed, 25 mm round

NTIMK032 / 19380

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.