MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Seals Eastern 5433 Nitrile Rubber
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: General purpose Nitrile; Low water swell

Information provided by Seals Eastern, Inc.

Key Words: NBR
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A >= 65>= 65ASTM D2240, Type A
 7575AVG; ASTM D2240, Type A
 73
@Treatment Temp. 100 °C,
Time 252000 sec
73
@Treatment Temp. 212 °F,
Time 70.0 hour
After Dry Heat Aging; ASTM D865
Tensile Strength at Break >= 16.87 MPa>= 2447 psiASTM D412 Method A
 21.64 MPa3138 psiAVG; ASTM D412 Method A
 22.826 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
3310.6 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM D865
Tensile Stress at Strain  0.669 MPa
@Strain 25 %
97.0 psi
@Strain 25 %
Average; ASTM D412 Method A
 >= 1.59 MPa
@Strain 50 %
>= 231 psi
@Strain 50 %
Minimum; ASTM D412 Method A
 2.10 MPa
@Strain 50 %
304 psi
@Strain 50 %
Average; ASTM D412 Method A
 >= 2.48 MPa
@Strain 100 %
>= 359 psi
@Strain 100 %
Minimum; ASTM D412 Method A
 3.96 MPa
@Strain 100 %
575 psi
@Strain 100 %
Average; ASTM D412 Method A
Elongation at Break >= 260 %>= 260 %ASTM D412 Method A
 379 %379 %AVG; ASTM D412 Method A
 367.6 %
@Treatment Temp. 100 °C,
Time 252000 sec
367.6 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM D865
Modulus of Elasticity 0.007874 GPa1.142 ksiASTM D412 Method A
Poissons Ratio 0.500.50Calculated
Shear Modulus 0.00263 GPa0.381 ksiASTM D412 Method A
Secant Modulus 0.007405 GPa1.074 ksiASTM D412 Method A
Tear Strength Test 324324(psi); ASTM D624, Die B
Compression Set  7.5 %
@Temperature 100 °C,
Time 79200 sec
7.5 %
@Temperature 212 °F,
Time 22.0 hour
ASTM D395, Test B
 10 %
@Temperature 100 °C,
Time 252000 sec
10 %
@Temperature 212 °F,
Time 70.0 hour
ASTM D395, Test B
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg -29.4 °C-21.0 °FASTM D1329
 
Descriptive Properties
Strain Energy / Unit Volume at 20% Elongation (psi)22

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Seals Eastern 5401 Nitrile Rubber
Seals Eastern 7202 Nitrile Rubber
Seals Eastern 5353 Nitrile Rubber
Seals Eastern 5400 Nitrile Rubber
Seals Eastern 5403 Nitrile Rubber

PSEAL07 / 80154

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.