MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

VICTREX HT™ G45 Polyetherketone
Categories: Polymer; Thermoplastic; Polyketone

Material Notes: Product Description: High performance thermoplastic material, unreinforced PolyEtherKetone (PEK), semi crystalline, depth filtered granules for injection moulding, low flow, FDA food contact compliant

Typical Application Areas: Applications for higher strength and stiffness as well as good ductility at higher temperatures. Chemically resistant to aggressive environments, suitable for sterilization for medical and food contact applications.

Information Provided by Victrex.

Key Words: PEK
Vendors: With over 30 years of focus, experience and security of supply Victrex Polymer Solutions is the world’s leading manufacturer of high performance Polyaryletherketones (PAEK) including versatile VICTREX™ PEEK. We work with our customers and end users to deliver technology driven solutions to meet the challenges and opportunities they face and help them to achieve new levels of cost savings, quality and performance. Visit www.victrex.com, call (800) VICTREX /1-484-342-6001, or email victrexplc@victrex.com.

Ensinger TECAPEEK™ shapes are manufactured exclusively with Victrex™ PEEK polymer. The Ensinger process and Victrex resins ensure reliability, consistency, dimensional stability, and high temperature mechanical performance.

Drake extrudes shapes and machines and injection molds parts in Torlon® PAI, PEEK, PAEK, Ryton PPS and Ultem PEI. It also machines Vespel® PI. Innovations include cryogenic CryoDyn® CT-200 shapes as a PCTFE alternative; efficient Seamless Tube® and the largest extruded rod diameters to >254mm and plate thicknesses to > 100mm. Certified to ISO 9001:2015 and AS9100D. Visit www.DrakePlastics.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.30 g/cc0.0470 lb/in³Crystalline; ISO 1183
Water Absorption at Saturation  0.60 %
@Temperature 23.0 °C
0.60 %
@Temperature 73.4 °F
ISO 62
 0.75 %
@Temperature 100 °C
0.75 %
@Temperature 212 °F
ISO 62
Viscosity 400000 cP
@Temperature 400 °C
400000 cP
@Temperature 752 °F
Melt; ISO 11443
Linear Mold Shrinkage, Flow 0.010 cm/cm0.010 in/in415°C nozzle, 220°C tool; ISO 294-4
Linear Mold Shrinkage, Transverse 0.012 cm/cm0.012 in/in415°C nozzle, 220°C tool; ISO 294-4
Spiral Flow 19.0 cm
@Thickness 1.00 mm
7.48 in
@Thickness 0.0394 in
Mold Temp: 220°C, Melt Temp: 4155°C; Victrex
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8686ISO 868
Tensile Strength, Yield 110 MPa16000 psiISO 527
Elongation at Break 35 %35 %ISO 527
Tensile Modulus 4.20 GPa609 ksiISO 527
Flexural Strength  16.0 MPa
@Temperature 275 °C
2320 psi
@Temperature 527 °F
ISO 178
 32.0 MPa
@Temperature 175 °C
4640 psi
@Temperature 347 °F
ISO 178
 105 MPa
@Temperature 125 °C
15200 psi
@Temperature 257 °F
ISO 178
 180 MPa
@Strain 3.5 %,
Temperature 23.0 °C
26100 psi
@Strain 3.5 %,
Temperature 73.4 °F
ISO 178
Flexural Yield Strength 180 MPa
@Temperature 23.0 °C
26100 psi
@Temperature 73.4 °F
ISO 178
Flexural Modulus 4.20 GPa609 ksiISO 178
Compressive Strength  30.0 MPa
@Temperature 200 °C
4350 psi
@Temperature 392 °F
ISO 604
 90.0 MPa
@Temperature 120 °C
13100 psi
@Temperature 248 °F
ISO 604
 140 MPa
@Temperature 23.0 °C
20300 psi
@Temperature 73.4 °F
ISO 604
Izod Impact, Notched (ISO) 7.00 kJ/m²3.33 ft-lb/in²ISO 180/A
Izod Impact, Unnotched (ISO) NBNBISO 180/U
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  1.00e+9 ohm-cm
@Temperature 275 °C
1.00e+9 ohm-cm
@Temperature 527 °F
IEC 60093
 1.00e+15 ohm-cm
@Temperature 125 °C
1.00e+15 ohm-cm
@Temperature 257 °F
IEC 60093
 1.00e+16 ohm-cm
@Temperature 23.0 °C
1.00e+16 ohm-cm
@Temperature 73.4 °F
IEC 60093
Dielectric Strength 17.0 kV/mm
@Thickness 2.00 mm
432 kV/in
@Thickness 0.0787 in
IEC 60243-1
Comparative Tracking Index 150 V150 V(450G); IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  45.0 µm/m-°C
@Temperature <=152 °C
25.0 µin/in-°F
@Temperature <=306 °F
Below Tg; ISO 11359
 75.0 µm/m-°C
@Temperature >=152 °C
41.7 µin/in-°F
@Temperature >=306 °F
Above Tg; ISO 11359
CTE, linear, Transverse to Flow  55.0 µm/m-°C
@Temperature <=152 °C
30.6 µin/in-°F
@Temperature <=306 °F
Below Tg; ISO 11359
 130 µm/m-°C
@Temperature >=152 °C
72.2 µin/in-°F
@Temperature >=306 °F
Above Tg; ISO 11359
Specific Heat Capacity 2.20 J/g-°C0.526 BTU/lb-°FDSC
Thermal Conductivity 0.290 W/m-K2.01 BTU-in/hr-ft²-°FAverage; ISO/CD 22007-4
 0.320 W/m-K2.22 BTU-in/hr-ft²-°FAlong Flow; ISO/CD 22007-4
Melting Point 373 °C703 °FISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 163 °C325 °FISO 75-f
Glass Transition Temp, Tg 152 °C306 °FOnset; ISO 11357
 160 °C320 °FMidpoint; ISO 11357-2
 
Processing PropertiesMetricEnglishComments
Processing Temperature <= 100 °C<= 212 °FHopper Temperature
Rear Barrel Temperature 390 °C734 °F
Middle Barrel Temperature 395 - 405 °C743 - 761 °F
Front Barrel Temperature 410 °C770 °F
Nozzle Temperature 415 °C779 °F
Mold Temperature 200 - 220 °C392 - 428 °F
Drying Temperature 120 - 150 °C248 - 302 °F
Dry Time 3.00 - 5.00 hour3.00 - 5.00 hour
 
Descriptive Properties
ColorNatural/Beige
Gate> 1mm or 0.5 x part thickness
RunnerDie/nozzle > 3mm, manifold > 3.5mm
Toxicity Index0.074CO content, NES 713
 0.15CO2, NES 712
 0.22Total gases, NES 712

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
VICTREX™ PEEK 450G™ General Purpose
VICTREX™ PEEK 450P Polyetheretherketone, Unreinforced
VICTREX™ WG101 Polyaryletherketone
Ravago Manufacturing Americas Hylon N1000EHL Nylon 66
Ravago Manufacturing Americas Hylon® N1000EHL Nylon 6/6 (DAM)

PVICTB09 / 122197

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.