MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Haynes Hastelloy® C-22® alloy, 40% cold worked sheet
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: HASTELLOY® C-22® alloy is a nickel-chromium-molybdenum-tungsten alloy with excellent overall corrosion resistance compared to other Ni-Cr-Mo alloys, including HASTELLOY C-276 and C-4 alloys and alloy 625. C-22 alloy has outstanding resistance to pitting, crevice corrosion, and stress corrosion cracking. It has excellent resistance to oxidizing aqueous media including wet chlorine and mixtures containing nitric acid or oxidizing acids with chloride ions. C-22 alloy offers optimum resistance to environments where reducing and oxidizing conditions are encountered in process streams. Because of such versatility it can be used where “upset” conditions are likely to occur or in multi-purpose plants. C-22 alloy has exceptional resistance to a wide variety of chemical process environments, including strong oxidizers such as ferric and cupric chlorides, chlorine, hot contaminated solutions (organic and inorganic), formic and acetic acids, acetic anhydride, and seawater and brine solutions. C-22 alloy resists the formation of grain-boundary precipitates in the weld heat-affected zone, thus making it suitable for most chemical process applications in the as-welded condition.

Product Forms: C-22 alloy is available in most common product forms: plate, sheet, strip, billet, bar, wire, covered electrodes, pipe, and tubing.

Applications:

  • Acetic Acid/Acetic Anhydride
  • Acid Etching
  • Cellophane Manufacturing
  • Chlorination Systems
  • Complex Acid Mixtures
  • Electro-Galvanizing Rolls
  • Expansion Bellows
  • Flue Gas Scrubber Systems
  • Geothermal Wells
  • HF Furnace Scrubbers
  • Incineration Scrubber Systems
  • Nuclear Fuel Reprocessing
  • Pesticide Production
  • Phosphoric Acid Production
  • Pickling Systems
  • Plate Heat Exchangers
  • Selective Leaching Systems
  • SO2 Cooling Towers
  • Sulfonation Systems
  • Tubular Heat Exchangers
  • Weld Overlay-Valves

Data provided by the manufacturer, Haynes International, Inc.

Key Words: ASME Section VIII, Division I. Plate, sheet, strip, bar, tubing, and pipe are covered by ASME SB-574, ASME B-575, ASME SB-619, ASME SB-622, ASME SB-626, ASTM B-574, ASTM B-575, ASTM B-619, ASTM B-622, and ASTM B-626. DIN specification is 17744 No. 2.4602 (all forms), TUV Werkstoffblatt 479 (all forms). C-22 alloy falls within the range of UNS N06022 but has a more restricted composition for improved performance.
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.69 g/cc0.314 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B  93
@Temperature 23.0 °C
93
@Temperature 73.4 °F
 95
@Temperature 23.0 °C
95
@Temperature 73.4 °F
Tensile Strength, Ultimate 1324 MPa192000 psi
Tensile Strength, Yield 1200 MPa
@Strain 0.2 %
174000 psi
@Strain 0.2 %
Elongation at Break 9.0 %9.0 %in 50.8 mm
Modulus of Elasticity 206 GPa29900 ksiheat-treated at 1121°C (2050°F), rapid quenched, plate
 145 GPa
@Temperature 982 °C
21000 ksi
@Temperature 1800 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 154 GPa
@Temperature 871 °C
22300 ksi
@Temperature 1600 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 163 GPa
@Temperature 760 °C
23600 ksi
@Temperature 1400 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 171 GPa
@Temperature 649 °C
24800 ksi
@Temperature 1200 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 177 GPa
@Temperature 538 °C
25700 ksi
@Temperature 1000 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 183 GPa
@Temperature 427 °C
26500 ksi
@Temperature 801 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 190 GPa
@Temperature 316 °C
27600 ksi
@Temperature 601 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 196 GPa
@Temperature 204 °C
28400 ksi
@Temperature 399 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 203 GPa
@Temperature 93.0 °C
29400 ksi
@Temperature 199 °F
heat-treated at 1121°C (2050°F), rapid quenched, plate
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.000114 ohm-cm
@Temperature 24.0 °C
0.000114 ohm-cm
@Temperature 75.2 °F
 0.000123 ohm-cm
@Temperature 100 °C
0.000123 ohm-cm
@Temperature 212 °F
 0.000124 ohm-cm
@Temperature 200 °C
0.000124 ohm-cm
@Temperature 392 °F
 0.000125 ohm-cm
@Temperature 300 °C
0.000125 ohm-cm
@Temperature 572 °F
 0.000126 ohm-cm
@Temperature 400 °C
0.000126 ohm-cm
@Temperature 752 °F
 0.000127 ohm-cm
@Temperature 500 °C
0.000127 ohm-cm
@Temperature 932 °F
 0.000128 ohm-cm
@Temperature 600 °C
0.000128 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.4 µm/m-°C
@Temperature 24.0 - 93.0 °C
6.89 µin/in-°F
@Temperature 75.2 - 199 °F
 12.4 µm/m-°C
@Temperature 24.0 - 204 °C
6.89 µin/in-°F
@Temperature 75.2 - 399 °F
 12.6 µm/m-°C
@Temperature 24.0 - 316 °C
7.00 µin/in-°F
@Temperature 75.2 - 601 °F
 13.3 µm/m-°C
@Temperature 24.0 - 427 °C
7.39 µin/in-°F
@Temperature 75.2 - 801 °F
 13.9 µm/m-°C
@Temperature 24.0 - 538 °C
7.72 µin/in-°F
@Temperature 75.2 - 1000 °F
 14.6 µm/m-°C
@Temperature 24.0 - 649 °C
8.11 µin/in-°F
@Temperature 75.2 - 1200 °F
 15.3 µm/m-°C
@Temperature 24.0 - 760 °C
8.50 µin/in-°F
@Temperature 75.2 - 1400 °F
 15.8 µm/m-°C
@Temperature 24.0 - 871 °C
8.78 µin/in-°F
@Temperature 75.2 - 1600 °F
 16.2 µm/m-°C
@Temperature 24.0 - 982 °C
9.00 µin/in-°F
@Temperature 75.2 - 1800 °F
Specific Heat Capacity  0.414 J/g-°C
@Temperature 52.0 °C
0.0989 BTU/lb-°F
@Temperature 126 °F
 0.423 J/g-°C
@Temperature 100 °C
0.101 BTU/lb-°F
@Temperature 212 °F
 0.444 J/g-°C
@Temperature 200 °C
0.106 BTU/lb-°F
@Temperature 392 °F
 0.460 J/g-°C
@Temperature 300 °C
0.110 BTU/lb-°F
@Temperature 572 °F
 0.476 J/g-°C
@Temperature 400 °C
0.114 BTU/lb-°F
@Temperature 752 °F
 0.489 J/g-°C
@Temperature 500 °C
0.117 BTU/lb-°F
@Temperature 932 °F
 0.514 J/g-°C
@Temperature 600 °C
0.123 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity  10.1 W/m-K
@Temperature 48.0 °C
70.1 BTU-in/hr-ft²-°F
@Temperature 118 °F
 11.1 W/m-K
@Temperature 100 °C
77.0 BTU-in/hr-ft²-°F
@Temperature 212 °F
 13.4 W/m-K
@Temperature 200 °C
93.0 BTU-in/hr-ft²-°F
@Temperature 392 °F
 15.5 W/m-K
@Temperature 300 °C
108 BTU-in/hr-ft²-°F
@Temperature 572 °F
 17.5 W/m-K
@Temperature 400 °C
121 BTU-in/hr-ft²-°F
@Temperature 752 °F
 19.5 W/m-K
@Temperature 500 °C
135 BTU-in/hr-ft²-°F
@Temperature 932 °F
 21.3 W/m-K
@Temperature 600 °C
148 BTU-in/hr-ft²-°F
@Temperature 1110 °F
Melting Point 1357 - 1399 °C2475 - 2550 °F
Solidus 1357 °C2475 °F
Liquidus 1399 °C2550 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.010 %<= 0.010 %
Chromium, Cr 22 %22 %
Cobalt, Co <= 2.5 %<= 2.5 %
Iron, Fe 3.0 %3.0 %
Manganese, Mn <= 0.50 %<= 0.50 %
Molybdenum, Mo 13 %13 %
Nickel, Ni 56 %56 %
Silicon, Si <= 0.080 %<= 0.080 %
Tungsten, W 3.0 %3.0 %
Vanadium, V <= 0.35 %<= 0.35 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals DURANICKEL® 301 (UNS N03301) Annealed and Aged Strip
Sandvik Sanicro 28 Billet
IN-792 Cast Nickel Superalloy
Haynes 230® alloy, cold rolled and 1232°C solution annealed sheet
Haynes 230® alloy, 10% cold reduction, 1121°C anneal for 5 minutes

NHC2BC / 17098

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.