MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celstran® PA66-GF30-02 Nylon 66, 30% Glass Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: 30% long glass fiber reinforced, heat stabilized, Nylon 6/6

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.36 g/cc1.36 g/ccASTM D792
Density 1.36 g/cc0.0491 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0010 - 0.0020 cm/cm0.0010 - 0.0020 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0030 - 0.0040 cm/cm0.0030 - 0.0040 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 170 MPa24700 psi5mm/min; ISO 527-2/1A
 194 MPa28100 psiASTM D638
 110 MPa
@Temperature 121 °C
16000 psi
@Temperature 250 °F
ASTM D638
 228 MPa
@Temperature -40.0 °C
33100 psi
@Temperature -40.0 °F
ASTM D638
Elongation at Break 2.1 %2.1 %5mm/min; ISO 527-2/1A
 2.4 %2.4 %ASTM D638
 2.5 %
@Temperature 4.44 °C
2.5 %
@Temperature 40.0 °F
ASTM D638
 2.7 %
@Temperature 121 °C
2.7 %
@Temperature 250 °F
ASTM D638
Tensile Modulus 9.70 GPa1410 ksi50mm/min; ISO 527-2/1A
 10.3 GPa1490 ksiASTM D638
 5.31 GPa
@Temperature 121 °C
770 ksi
@Temperature 250 °F
ASTM D638
 9.31 GPa
@Temperature -40.0 °C
1350 ksi
@Temperature -40.0 °F
ASTM D638
Flexural Strength 280 MPa40600 psiISO 178
 290 MPa42100 psiASTM D790
 159 MPa
@Temperature 121 °C
23000 psi
@Temperature 250 °F
ASTM D790
 298 MPa
@Temperature -40.0 °C
43200 psi
@Temperature -40.0 °F
ASTM D790
Flexural Modulus 9.00 GPa1310 ksiISO 178
 9.10 GPa1320 ksiASTM D790
 4.41 GPa
@Temperature 121 °C
640 ksi
@Temperature 250 °F
ASTM D790
 9.38 GPa
@Temperature -40.0 °C
1360 ksi
@Temperature -40.0 °F
ASTM D790
Izod Impact, Notched 2.67 J/cm5.00 ft-lb/inASTM D256
 2.99 J/cm
@Temperature -40.0 °C
5.60 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 3.84 J/cm
@Temperature 149 °C
7.20 ft-lb/in
@Temperature 300 °F
ASTM D256
Charpy Impact, Notched 2.30 J/cm²10.9 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 252 °C485 °FASTM D648
 252 °C486 °FISO 75-1, -2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 - 100 °C176 - 212 °Fcavity
Feed Temperature 20.0 - 50.0 °C68.0 - 122 °F
Zone 1 285 - 295 °C545 - 563 °F
Zone 2 290 - 300 °C554 - 572 °F
Zone 3 300 - 310 °C572 - 590 °F
Zone 4 300 - 315 °C572 - 599 °F
Die Temperature 300 - 315 °C572 - 599 °F
Melt Temperature 300 - 315 °C572 - 599 °F
Drying Temperature 70.0 - 80.0 °C158 - 176 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Moisture Content <= 0.18 %<= 0.18 %
 
Descriptive Properties
Injection moldingYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
EMS-Grivory Grilon® AG-30 PA66-GF30
Celanese Celstran® PA66-GF30-07 Nylon 66, 30% Glass Reinforced
Envalior Akulon® S223-HG6 PA66-GF30, Conditioned, 30% Glass Filled, Heat Stabilized
Envalior Novamid® 3021GH30 NAT PA66-GF30
Celanese Zytel® 70G30L NC010 PA66-GF30

PHCQ161 / 178616

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.