MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior EcoPaXX® Q-HG6 PA410-GF30
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: 30% Glass Reinforced, Heat Stabilized

EcoPaXX® is a former DSM Engineering Plastics product line now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.34 g/cc0.0484 lb/in³dry; ISO 1183
Moisture Absorption 1.50 %1.50 %Sim. To ISO 62
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.010 cm/cm0.010 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 115 MPa16700 psicond; ISO 527-1/-2
 170 MPa24700 psidry; ISO 527-1/-2
Elongation at Break 4.0 %4.0 %dry; ISO 527-1/-2
 5.8 %5.8 %cond; ISO 527-1/-2
Tensile Modulus 7.00 GPa1020 ksicond; ISO 527-1/-2
 9.50 GPa1380 ksidry; ISO 527-1/-2
Flexural Strength 185 MPa26800 psicond; ISO 178
 260 MPa37700 psidry; ISO 178
Flexural Modulus 6.30 GPa914 ksicond; ISO 178
 8.50 GPa1230 ksidry; ISO 178
Charpy Impact Unnotched  6.00 J/cm²
@Temperature -30.0 °C
28.6 ft-lb/in²
@Temperature -22.0 °F
dry; ISO 179/1eU
 8.00 J/cm²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eU
 8.00 J/cm²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eU
Charpy Impact, Notched  0.900 J/cm²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
dry; ISO 179/1eA
 1.10 J/cm²
@Temperature 23.0 °C
5.23 ft-lb/in²
@Temperature 73.4 °F
dry; ISO 179/1eA
 1.50 J/cm²
@Temperature 23.0 °C
7.14 ft-lb/in²
@Temperature 73.4 °F
cond; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmcond; IEC 60093
 1.00e+14 ohm-cm1.00e+14 ohm-cmdry; IEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmcond; IEC 60093
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 32.0 µm/m-°C17.8 µin/in-°Fdry; ISO 11359-1/-2
CTE, linear, Transverse to Flow 66.0 µm/m-°C36.7 µin/in-°Fdry; ISO 11359-1/-2
Melting Point 250 °C482 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 243 °C469 °Fdry; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 215 °C419 °Fdry; ISO 75-1/-2
 
Descriptive Properties
Calculated Bio Based Carbon Content (%)70ASTM 6866

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Envalior EcoPaXX® Q-HG10 PA410-GF50
RTP Company RTP 2099 X 121249 C Bio-Based Polylactic Acid (PLA); Standard Nucleator - Glass Fiber - 68% Renewable Resource Content
BASF Ultramid® A3WG6 30% Glass Filled PA66 (Conditioned)
Ashley Polymers Ashlene® 68MG Nylon 66, Glass/Mineral reinforced
A. Schulman ComAlloy Voloy® 682 Nylon 6/6, Glass Fiber, Nylon 6/6 Alloy, Flame Retardant, UL

PDSM9829 / 161450

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.